Steel Files: Forged, Cut and Hardened

A file is a bar of high-carbon steel, about 1.0–1.25 % carbon, covered in rows of tiny chisel cuts. The blank is forged with a tang, annealed soft, ground flat, and the teeth are raised one by one with a chisel and hammer: each blow cuts a groove and lifts its edge into a tooth. A single-cut file has one row of parallel cuts, at 65–85° to the length; a double-cut file has a second row crossing the first, for general work the first at 40–45° and the second at 70–80°. The file is then hardened as hard as it will go by quenching it in cold brine, and is never tempered; only the tang is softened so it will not snap. Factories do the same steps by machine.
Abantado
2 days (annealing overnight)

Mga Tagubilin

1

Forge the blank

At a yellow heat, draw the high-carbon steel to the file's section and forge a narrow, pointed tang at one end.

Mga materyales para sa hakbang na ito:

Bilyeta ng aserong mataas sa karbonBilyeta ng aserong mataas sa karbon0.5 kg

Mga kailangang kasangkapan:

Pandayan ng pandayPandayan ng panday
PalihanPalihan
Martilyong PampandayMartilyong Pampanday
Sipit ng PandaySipit ng Panday
2

Anneal

Heat the blank no hotter than a blood-red and let it cool very slowly, shut away from the air; factories leave blanks in closed boxes in the furnace for 24–36 hours. Cooled in open air it would harden again.

Mga kailangang kasangkapan:

Pandayan ng pandayPandayan ng panday
3

Straighten and grind

Straighten the blank, grind off the scale and make the faces flat and even, or the teeth will not be uniform.

Mga kailangang kasangkapan:

Batong panghasang gulongBatong panghasang gulong
4

Cut the teeth

Hold the chisel at an angle and strike it, then move it a small, regular distance and strike again; each blow raises one tooth. For a double cut, cut the first row (overcut), then a second row crossing it (upcut). To cut the other face, turn the file over on a pewter plate so the finished teeth are not crushed.

Mga kailangang kasangkapan:

Pait na panggawa ng ngipin ng kikilPait na panggawa ng ngipin ng kikil
Martilyong PampandayMartilyong Pampanday
PalihanPalihan
Plaka ng peltrePlaka ng peltre
5

Harden

Heat the file evenly to its hardening heat and plunge it into a bath of cold brine, which cools faster than water and leaves it harder. Do not temper it.

Mga materyales para sa hakbang na ito:

AsinAsin1 kg

Mga kailangang kasangkapan:

Pandayan ng pandayPandayan ng panday
BaldeBalde
Sipit ng PandaySipit ng Panday
6

Soften the tang

Reheat the tang alone so it is no longer glass-hard: a fully hard tang snaps when the handle is driven on. Clean and oil the file.

Mga kailangang kasangkapan:

Pandayan ng pandayPandayan ng panday
Sipit ng PandaySipit ng Panday

Mga Materyales

2

Mga Kinakailangang Kasangkapan

8

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...