Nichrome Wire: Nickel and Chromium Fused, Drawn and Annealed
Forge

Nilikha ni

Forge

18. Oktubre 2026NO
16
0
0
3
0

Nichrome Wire: Nickel and Chromium Fused, Drawn and Annealed

Nichrome is the heating wire of toasters and irons. Albert Marsh patented it in 1906: nickel with less than 25 % chromium, drawn into wire and annealed, with about fifty times the resistance of copper and great resistance to oxidation when hot. Iron, he wrote, will not do. Elwood Haynes (1907) fused pure, carbon-free nickel and chromium in a magnesia crucible under an oxyhydrogen flame. White heat: face shield and gloves. The picture: Marsh's patent drawing, a rheostat wound with the alloy (US 811,859).
Abantado
3 days

Mga Tagubilin

1

Weigh 85 nickel to 15 chromium

Cut 85 g of nickel sheet into small pieces and weigh 15 g of chromium: Marsh's own example. Both must be pure and free of carbon.

Mga materyales para sa hakbang na ito:

Manipis na nikelManipis na nikel85 g
Metal na KromyumMetal na Kromyum15 g

Mga kailangang kasangkapan:

Panggunting ng metalPanggunting ng metal
Timbangang panimbangTimbangang panimbang
2

Fuse under the oxyhydrogen flame

Put the metals in a magnesia crucible, set it in a furnace lined with magnesia, and heat it with the oxyhydrogen blowpipe until both have melted together.

Mga kailangang kasangkapan:

Krusibol na MagnesiaKrusibol na Magnesia
Oksido ng magnesiyoOksido ng magnesiyo
Oksihidrohenong BlowpipeOksihidrohenong Blowpipe
Sipit ng KrisolSipit ng Krisol
Panangga sa MukhaPanangga sa Mukha
Gwantes na KatadGwantes na Katad
3

Cast a rod

Pour the alloy into a narrow mould to get a rod that will start in the largest hole of the drawplate.

Mga kailangang kasangkapan:

Hulmahan ng lingoteHulmahan ng lingote
Sipit ng KrisolSipit ng Krisol
Panangga sa MukhaPanangga sa Mukha
Gwantes na KatadGwantes na Katad
4

Draw and anneal

Draw the rod down through the drawplate one hole at a time, as in the drawplate blueprint, and anneal it in the furnace whenever it gets hard. Marsh gives no annealing temperature. Stop at 0.41 mm (0.016 in).

Mga kailangang kasangkapan:

Plakang panghila ng kawad na aseroPlakang panghila ng kawad na asero
Panipit na panghilaPanipit na panghila
Pampadulas sa paghila ng kawadPampadulas sa paghila ng kawad
Pugon na UlingPugon na Uling
MikrometroMikrometro
Gwantes na KatadGwantes na Katad
5

Check the resistance

Measure one metre with the multimeter. Marsh's 15 % wire of this size measured about 2.3 ohms per foot, which is 7.5 ohms per metre.

Mga kailangang kasangkapan:

MultimetroMultimetro

Mga Materyales

2

Mga Kinakailangang Kasangkapan

15

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...