Oriented Strontium Ferrite Disc Magnet: Agate-Milled, 10,000 Oersted Field (Gorter, Philips 1956, Ex. 8)

A strontium ferrite magnet oriented in a magnetic field: strontium carbonate and iron oxide milled, pre-fired 2 hours at 1000 °C, ground fine in an agate mill, then oriented, heated and sintered as in Example 4. In the principal direction it held 2,640 gauss with a coercive force of 2,825 oersted and a (BH)max of 1.63 × 10⁶. Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 8. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
3 days

Mga Tagubilin

1

Weigh strontium carbonate and iron oxide

Weigh 29.5 g strontium carbonate and 179 g ferric oxide.

Mga materyales para sa hakbang na ito:

Strontium carbonateStrontium carbonate29.5 g
Ferric oxideFerric oxide179 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Panala sa Hininga na P100Panala sa Hininga na P100
2

Mill 15 hours with alcohol, dry

Grind in a ball mill with alcohol for 15 hours. Remove the alcohol and dry the powder.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
3

Pre-fire 2 hours at 1000 °C in air

Heat the powder for 2 hours at 1000 °C in an electric furnace in air. Let it cool.

Mga kailangang kasangkapan:

Muffle furnaceMuffle furnace
Krisol na may takip (porselana)Krisol na may takip (porselana)
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Grind 4 hours in an agate centrifugal mill

Grind the cooled material for 4 hours with alcohol in an agate centrifugal mill, then dry it. This is the pre-fired powder.

Mga kailangang kasangkapan:

Centrifugal na gilingang agataCentrifugal na gilingang agata
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
5

Stir into 8 % polyvinyl acetate in acetone

Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 1 cc of solution per gram of powder. The binder burns off later.

Mga kailangang kasangkapan:

Polyvinyl acetatePolyvinyl acetate
AcetoneAcetone
Timbangang panimbangTimbangang panimbang
6

Orient in a 10000 oersted field

Put the suspension in a moulding die between the poles of a magnet and apply a first field of 10000 oersted. Remove the binder solution while the field is on.

Mga kailangang kasangkapan:

Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
ElektromagnetoElektromagneto
Haydroliko na pandiinHaydroliko na pandiin
7

Heat to 500 °C in a 2000 oersted field

Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
ElektromagnetoElektromagneto
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
8

Sinter: through a 1280 °C zone in 5 minutes

Pass the block at 20 mm per minute through an electric furnace in air at 1280 °C with a 10 cm hot zone: about 5 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
9

Magnetise in the principal direction

Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

2

Mga Kinakailangang Kasangkapan

17

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...