Precipitated Silica: Hot Water Glass Carbonated, Then Acidified to pH 6.75 (Allen 1957)
Youblob · CC0
Charlie

Nilikha ni

Charlie

27. Oktubre 2026DE
13
0
0
0
0

Precipitated Silica: Hot Water Glass Carbonated, Then Acidified to pH 6.75 (Allen 1957)

Bubble carbon dioxide through hot dilute water glass and the silica comes down as an extremely fine white powder rather than a gel. Edward Allen of Columbia-Southern made it this way as a white reinforcing filler for rubber; this follows his Example XI, which gave a powder of 148 m² per gram. Source: E. M. Allen (Columbia-Southern), US 2,805,955 (1957), Example XI. The percentages are our arithmetic; the filter, mill and indicator are ours. Picture drawn by Youblob.
Katamtaman
2 days

Mga Tagubilin

1

Dilute the water glass

Take 12,850 g of sodium silicate solution holding 976 g Na2O and 3115 g SiO2 (7.6 % and 24.2 %, a silica to soda ratio of 3.19 by weight; our arithmetic). Dilute it with water to 48 litres in a stirred kettle with a heating coil and thermometer, and heat to 95 °C.

Mga materyales para sa hakbang na ito:

Water glass (sodium silicate na solusyon)Water glass (sodium silicate na solusyon)12850 g
TubigTubig1 as required

Mga kailangang kasangkapan:

Reactor na may presyonReactor na may presyon
PanghaloPanghalo
TermometroTermometro
Timbangang panimbangTimbangang panimbang
2

Carbonate for an hour

Bubble in pure carbon dioxide fast enough to add the theoretical amount in about 30 minutes, and keep going at that rate for about 1 hour. The slurry ends at pH 9.85.

Mga kailangang kasangkapan:

Gas na carbon dioxideGas na carbon dioxide
Reactor na may presyonReactor na may presyon
PanghaloPanghalo
TermometroTermometro
Papel na panukat ng pHPapel na panukat ng pH
3

Filter and wash

Filter the slurry and wash the cake twice with hot water.

Mga materyales para sa hakbang na ito:

TubigTubig1 as required

Mga kailangang kasangkapan:

Embudong Büchner (porselana)Embudong Büchner (porselana)
Papel na PansalaPapel na Pansala
4

Acidify to pH 6.75

Stir the cake back into water and bring it to pH 6.75 with 400 ml of 3.5 N hydrochloric acid.

Mga materyales para sa hakbang na ito:

TubigTubig1 as required

Mga kailangang kasangkapan:

Hydrochloric acidHydrochloric acid
Sisidlang salaminSisidlang salamin
PanghaloPanghalo
Papel na panukat ng pHPapel na panukat ng pH
5

Wash out the chloride

Filter again and wash the cake with hot water until it is nearly free of chloride.

Mga materyales para sa hakbang na ito:

TubigTubig1 as required

Mga kailangang kasangkapan:

Embudong Büchner (porselana)Embudong Büchner (porselana)
Papel na PansalaPapel na Pansala
6

Dry at 105 °C and grind

Dry it at 105 °C in a fan oven and grind it to a fine powder. Allen's had a pH of 8.2, 0.61 % sodium and a surface area of 148 m² per gram.

Mga kailangang kasangkapan:

Hurnong pantuyoHurnong pantuyo
Almires at PanghaloAlmires at Panghalo
Garapong Salamin na May TakipGarapong Salamin na May Takip

Mga Materyales

2

Mga Kinakailangang Kasangkapan

13

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...