Screwdriver: a Flat Blade Forged, Packed at a Low Heat and Tempered Grey (Holford, 1907)
Forge

Nilikha ni

Forge

4. Nobyembre 2026NO
2
0
0
0
0

Screwdriver: a Flat Blade Forged, Packed at a Low Heat and Tempered Grey (Holford, 1907)

A flat screwdriver is a steel shank flattened to a blade that fits the slot of a screw. H. Holford's 20th Century Toolsmith and Steelworker (1907) says most smiths make them so they twist or break on a hard screw, and gives his cure: forge it from 75-point carbon steel, strike the blade a few good blows on each flat at a low heat, harden it and let the temper run to grey. His Fig. 60 shows the shape without its handle. He gives no sizes and no handle, which are unknown here; the brine bath is from his chapter on the hardening bath. Source: H. Holford (1907), pp. 21, 118. Picture: his Fig. 60.
Katamtaman
Half a day

Mga Tagubilin

1

Read Holford

"Strike it a few good blows on each flat side of the screw driving edge while at a low heat. Then harden and allow the temper to draw to a grey, cool off and you will have a screw driver that will give unlimited satisfaction."
2

Forge the shape

Take good steel of 75 points carbon. Forge it to the shape of Fig. 60: a round shank, flattened at one end to the driving blade and drawn to a pointed tang at the other for the handle. Holford gives no sizes (unknown).

Mga materyales para sa hakbang na ito:

Parisukat na barang tool steelParisukat na barang tool steel1 bar

Mga kailangang kasangkapan:

PandayanPandayan
PalihanPalihan
Martilyo ng pandayMartilyo ng panday
Sipit ng pandaySipit ng panday
Hindi alam na sukatHindi alam na sukat
Salaming pangkaligtasanSalaming pangkaligtasan
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
3

Pack the blade

At a low heat, strike a few good blows on each flat side of the driving edge.

Mga kailangang kasangkapan:

Martilyo ng pandayMartilyo ng panday
PalihanPalihan
PandayanPandayan
Sipit ng pandaySipit ng panday
4

Harden and temper grey

Heat the blade end evenly and quench it in the hardening bath. Holford's bath is clean water free from grease, best made into a brine with as much salt as the water will dissolve, kept as large and as cold as possible. Brighten the blade with a file so the colours show, draw the temper to a grey, then cool it off.

Mga kailangang kasangkapan:

PandayanPandayan
Puspos na solusyon ng asinPuspos na solusyon ng asin
Sipit ng pandaySipit ng panday
Pinong kikilPinong kikil
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
5

Fit a handle

Fit a handle on the tang. Holford shows the screwdriver without one and does not say what it is made of (unknown).

Mga materyales para sa hakbang na ito:

Hindi kilalang materyalHindi kilalang materyal1 handle
6

History and honest limits

Holford, a toolsmith writing for blacksmiths and tool dressers, says a good screwdriver is prized by every mechanic, woodworkers most of all, yet few smiths could make one that would not break or twist. His temper table lists the screwdriver at grey, in 0.75 carbon steel. He gives no sizes, no handle and no heat for hardening; those are unknown here, and the tools are ours.

Mga Materyales

2

Mga Kinakailangang Kasangkapan

9

Ang blueprint na ito ay gumagawa ng

Kaugnay na Blueprint

Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.