Silver Solder from Fine Silver, Copper and Spelter: Gee, 1877

Silver solder joins silver, copper and brass with a strong, hard seam. The silversmith George Gee preferred one made of fine silver, shot copper and a little spelter (zinc), melted only once: his best hard solder is 16 dwt of fine silver, 3 dwt 12 gr of shot copper and 12 gr of spelter to the ounce, about 80, 17.5 and 2.5 per cent. More copper and zinc make it flow sooner (his medium, easy and common solders). Silver and copper alone give the hardest, least fusible solder; too much zinc makes it eat away during soldering.
Katamtaman
Two hours

Mga Tagubilin

1

Weigh the metals

Naglo-load ng Jupyter notebook…

Mga materyales para sa hakbang na ito:

Purong PilakPurong Pilak80 g
Lingote ng TansoLingote ng Tanso17.5 g
Lingote ng SinkLingote ng Sink2.5 g

Mga kailangang kasangkapan:

TimbanganTimbangan
Pait na pambakalPait na pambakal
2

Anneal and test the crucible

Before a new plumbago (graphite) crucible is charged, heat it slowly to redness on a fire that is dying down and has no blaze, so it does not crack. Touch it with a cold iron bar: if cracks show, reject it.

Mga kailangang kasangkapan:

Krisol na grapito at luwadKrisol na grapito at luwad
Pugon na UlingPugon na Uling
Sipit ng KrisolSipit ng Krisol
3

Melt silver and copper

Put the copper at the bottom of the crucible, the silver on top, and melt them in the furnace. Stir them well together with an iron stirrer, tapered at the point and first heated to redness. When the metals are just beginning to fuse, cover the melt with finely divided, pure charcoal to keep the air off it.

Mga materyales para sa hakbang na ito:

Uling - pinong durogUling - pinong durog1 as required

Mga kailangang kasangkapan:

Pugon na UlingPugon na Uling
Patulis na panghalong bakalPatulis na panghalong bakal
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Add the spelter

Hold the spelter in a long pair of tongs over the mouth of the crucible, inside the furnace, until it has almost reached its melting point, then drop it into the molten metal and stir quickly so it mixes in. Zinc burns away quickly in the air, so it goes in last.

Mga kailangang kasangkapan:

SipitSipit
Patulis na panghalong bakalPatulis na panghalong bakal
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
5

Pour the ingot

Withdraw the crucible from the furnace at once and pour into an ingot mould that is clean, smooth, lightly greased, dusted with fine charcoal and warmed: a cold mould makes the metal spout, but do not overheat it either. Melt solder only once; Gee found that solders containing volatile metals grow hard, brittle and drossy with repeated melting.

Mga materyales para sa hakbang na ito:

Uling - pinong durogUling - pinong durog1 as required

Mga kailangang kasangkapan:

Sipit ng KrisolSipit ng Krisol
Hulmahan ng lingoteHulmahan ng lingote
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
6

Roll into pallions or file to dust

Roll the solder out thin between flattening rollers and cut it lengthways and then crossways with hand shears into little bits (pallions), or file it into fine dust, according to the work in hand. The work is then bound together, wetted with a paste of borax and water, and the pallions laid on the joints and melted with a blowpipe flame.

Mga kailangang kasangkapan:

Makinang panipis ng metalMakinang panipis ng metal
Panggunting ng metalPanggunting ng metal
Kikil (Kikil na Pangkamay)Kikil (Kikil na Pangkamay)

Mga Materyales

4

Mga Kinakailangang Kasangkapan

12

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...