Strontium-Calcium Ferrite Disc Magnet: 0.06 mol SrCO3 and 0.04 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 24)
A strontium ferrite with 0.06 mol strontium carbonate and 0.04 mol calcium carbonate to 0.6 mol iron oxide, made as in Example 23. Went's rod held 2,120 gauss with a coercive force of 1,950 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 24. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days
Mga Tagubilin
1
1
Weigh the carbonates and iron oxide
Weigh the carbonates and iron oxide
Weigh 8.86 g strontium carbonate (0.06 mol), 4.004 g calcium carbonate (0.04 mol), 95.55 g ferric oxide (0.6 mol). The patent prints 81.86 g of strontium carbonate beside 0.06 mol. 0.06 mol is 8.86 g (ours, at 147.63 g per mol), the weight used here.
Mga materyales para sa hakbang na ito:
Strontium carbonate8.86 g
Calcium carbonate (puting tisa)4.004 g
Ferric oxide95.55 gMga kailangang kasangkapan:
Timbangang panimbang
Panala sa Hininga na P1002
2
Mill with alcohol 4 hours, dry
Mill with alcohol 4 hours, dry
As in Example 23: grind the mixture with alcohol in a ball mill for 4 hours, then dry it.
Mga kailangang kasangkapan:
Gilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %
Hurnong pantuyo3
3
Press at 1.5 t/cm²
Press at 1.5 t/cm²
Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).
Mga kailangang kasangkapan:
Haydroliko na pandiin
Hulmahan sa pagpindot ng disk4
4
Pass through a 1280 °C zone in 10 minutes
Pass through a 1280 °C zone in 10 minutes
Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.
Mga kailangang kasangkapan:
Hurnong Tubo
Guwantes na Matibay sa Init5
5
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Mga kailangang kasangkapan:
Elektromagneto
KompasMga Materyales
3- 8.86 gPlaceholder
- Placeholder
- 95.55 gPlaceholder
Mga Kinakailangang Kasangkapan
11- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Ang blueprint na ito ay gumagawa ng
Kaugnay na Blueprint
Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo
CC0 Pampublikong Domain
Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.
Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.