Strontium-Calcium Ferrite Disc Magnet: Equal Strontium and Calcium, 1280 °C (Went, Philips 1956, Ex. 27)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
5
0
0
0
0

Strontium-Calcium Ferrite Disc Magnet: Equal Strontium and Calcium, 1280 °C (Went, Philips 1956, Ex. 27)

A ferrite with half the strontium replaced by calcium: 0.3 mol strontium carbonate and 0.3 mol calcium carbonate to 3.1 mol iron oxide, milled 15 hours, pressed and passed through a 1280 °C furnace in 10 minutes. Went's rod held 1,645 gauss with a coercive force of 2,460 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 27. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days

Mga Tagubilin

1

Weigh the carbonates and iron oxide

Weigh 44.3 g strontium carbonate (0.3 mol), 30.2 g calcium carbonate (0.3 mol), 500.0 g ferric oxide (3.1 mol).

Mga materyales para sa hakbang na ito:

Strontium carbonateStrontium carbonate44.3 g
Calcium carbonate (puting tisa)Calcium carbonate (puting tisa)30.2 g
Ferric oxideFerric oxide500 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Panala sa Hininga na P100Panala sa Hininga na P100
2

Mill with alcohol 15 hours, dry

Grind the mixture with alcohol in a ball mill for 15 hours, then dry it.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
3

Press at 1.5 t/cm²

Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).

Mga kailangang kasangkapan:

Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
4

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

3

Mga Kinakailangang Kasangkapan

11

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...