Strontium Ferrite Disc Magnet: Presintered, 4 Minutes at 1150 °C (Went, Philips 1956, Ex. 25)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
1
0
0
0
0

Strontium Ferrite Disc Magnet: Presintered, 4 Minutes at 1150 °C (Went, Philips 1956, Ex. 25)

A strontium ferrite with more strontium: 0.4 mol strontium carbonate to 0.8 mol iron oxide, milled, presintered at 1000 °C, milled again, pressed and passed through a 1150 °C furnace in 4 minutes. Went's rod held 1,200 gauss with a coercive force of 3,710 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 25. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days

Mga Tagubilin

1

Dry the strontium carbonate and weigh

Dry the strontium carbonate at 100 °C. Weigh 59.05 g of it (0.4 mol) and 127.5 g ferric oxide (0.8 mol).

Mga materyales para sa hakbang na ito:

Strontium carbonateStrontium carbonate59.05 g
Ferric oxideFerric oxide127.5 g

Mga kailangang kasangkapan:

Hurnong pantuyoHurnong pantuyo
Timbangang panimbangTimbangang panimbang
Panala sa Hininga na P100Panala sa Hininga na P100
2

Mill 7 hours, dry at 110 °C

Grind with alcohol in a ball mill for 7 hours and dry at 110 °C.

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
3

Presinter in air at 1000 °C for 4 hours

Fire in air at 1000 °C for 4 hours.

Mga kailangang kasangkapan:

Muffle furnaceMuffle furnace
Krisol na may takip (porselana)Krisol na may takip (porselana)
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Mill again, dry, press at 1.5 t/cm²

Grind again 7 hours with alcohol, dry at 110 °C and press at 1.5 tonnes per cm² (ours: discs).

Mga kailangang kasangkapan:

Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
Hurnong pantuyoHurnong pantuyo
Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
5

Pass through a 1150 °C zone in 4 minutes

Sinter at 1150 °C by passing the pieces through a 4 cm hot zone at 10 mm per minute: 4 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

2

Mga Kinakailangang Kasangkapan

14

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...