Strontium Ferrite Disc Magnet: Presintered at 1100 °C, 0.2 mol SrCO3 to 1.1 mol Iron Oxide (Went, Philips 1956, Ex. 7)
A strontium ferrite: 0.2 mol strontium carbonate to 1.1 mol iron oxide, dried, milled, presintered 3.5 hours at 1100 °C, bound, formed and passed through a 1280 °C furnace in 10 minutes. Went's rod held 2,155 gauss with a coercive force of 2,500 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 7. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days
Mga Tagubilin
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 29.5 g strontium carbonate (0.2 mol) and 176.1 g ferric oxide (1.1 mol).
Mga materyales para sa hakbang na ito:
Strontium carbonate29.5 g
Ferric oxide176.1 gMga kailangang kasangkapan:
Timbangang panimbang
Panala sa Hininga na P1002
2
Dry at 200 °C, mill with alcohol 4 hours
Dry at 200 °C, mill with alcohol 4 hours
Dry the mixture at 200 °C, then grind it with alcohol in a ball mill for 4 hours and dry it.
Mga kailangang kasangkapan:
Hurnong pantuyo
Gilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %3
3
Presinter in air at 1100 °C for 3.5 hours
Presinter in air at 1100 °C for 3.5 hours
Fire the powder in air at 1100 °C for about 3.5 hours.
Mga kailangang kasangkapan:
Muffle furnace
Krisol na may takip (porselana)
Sipit ng Krisol
Guwantes na Matibay sa Init4
4
Add a binder and form, dry overnight
Add a binder and form, dry overnight
Add a binder as in Example 1 (polyvinyl alcohol or nitrocellulose). The patent extrudes rods; ours: press discs at 1.5 tonnes per cm². Dry overnight.
Mga kailangang kasangkapan:
Pulbos na polyvinyl alcohol
Haydroliko na pandiin
Hulmahan sa pagpindot ng disk
Hurnong pantuyo5
5
Pass through a 1280 °C zone in 10 minutes
Pass through a 1280 °C zone in 10 minutes
Sinter in air at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.
Mga kailangang kasangkapan:
Hurnong Tubo
Guwantes na Matibay sa Init6
6
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Mga kailangang kasangkapan:
Elektromagneto
KompasMga Materyales
2- 29.5 gPlaceholder
- 176.1 gPlaceholder
Mga Kinakailangang Kasangkapan
15- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Ang blueprint na ito ay gumagawa ng
Kaugnay na Blueprint
Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo
CC0 Pampublikong Domain
Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.
Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.