Strontium Ferrite Disc Magnet: Presintered at 1100 °C, 0.1 mol SrCO3 to 0.7 mol Iron Oxide (Went, Philips 1956, Ex. 8)
Charlie

Nilikha ni

Charlie

28. Oktubre 2026DE
5
0
0
0
0

Strontium Ferrite Disc Magnet: Presintered at 1100 °C, 0.1 mol SrCO3 to 0.7 mol Iron Oxide (Went, Philips 1956, Ex. 8)

A strontium ferrite: 0.1 mol strontium carbonate to 0.7 mol iron oxide, dried, milled, presintered 3.5 hours at 1100 °C, bound, formed and passed through a 1280 °C furnace in 10 minutes. Went's rod held 1,535 gauss with a coercive force of 2,800 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 8. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Abantado
2 days

Mga Tagubilin

1

Weigh strontium carbonate and iron oxide

Weigh 14.8 g strontium carbonate (0.1 mol) and 112.1 g ferric oxide (0.7 mol).

Mga materyales para sa hakbang na ito:

Strontium carbonateStrontium carbonate14.8 g
Ferric oxideFerric oxide112.1 g

Mga kailangang kasangkapan:

Timbangang panimbangTimbangang panimbang
Panala sa Hininga na P100Panala sa Hininga na P100
2

Dry at 200 °C, mill with alcohol 4 hours

Dry the mixture at 200 °C, then grind it with alcohol in a ball mill for 4 hours and dry it.

Mga kailangang kasangkapan:

Hurnong pantuyoHurnong pantuyo
Gilingang Bolang BakalGilingang Bolang Bakal
Etanol - antas laboratoryo, 95 %Etanol - antas laboratoryo, 95 %
3

Presinter in air at 1100 °C for 3.5 hours

Fire the powder in air at 1100 °C for about 3.5 hours.

Mga kailangang kasangkapan:

Muffle furnaceMuffle furnace
Krisol na may takip (porselana)Krisol na may takip (porselana)
Sipit ng KrisolSipit ng Krisol
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
4

Add a binder and form, dry overnight

Add a binder as in Example 1 (polyvinyl alcohol or nitrocellulose). The patent extrudes rods; ours: press discs at 1.5 tonnes per cm². Dry overnight.

Mga kailangang kasangkapan:

Pulbos na polyvinyl alcoholPulbos na polyvinyl alcohol
Haydroliko na pandiinHaydroliko na pandiin
Hulmahan sa pagpindot ng diskHulmahan sa pagpindot ng disk
Hurnong pantuyoHurnong pantuyo
5

Pass through a 1280 °C zone in 10 minutes

Sinter in air at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Mga kailangang kasangkapan:

Hurnong TuboHurnong Tubo
Guwantes na Matibay sa InitGuwantes na Matibay sa Init
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Mga kailangang kasangkapan:

ElektromagnetoElektromagneto
KompasKompas

Mga Materyales

2

Mga Kinakailangang Kasangkapan

15

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.