Tinned Copper Saucepan, Raised from Sheet and Riveted
A copper saucepan heats evenly; lined with tin, it keeps the copper away from the food. Raise a copper disc into a pan over the stake, anneal it whenever it stiffens, rivet on an iron handle, then tin the inside as Andrew Ure (1839) describes: scour, heat, rub with sal ammoniac, melt tin with rosin on it and wipe it over with tow.
The picture: copper saucepans with riveted iron handles in the kitchen of Bourbilly Castle, Burgundy.
Abantado
Two days
Mga Tagubilin
1
1
Cut and raise
Cut and raise
Cut a disc from copper sheet. Hammer it down into a hollow in a wooden block, then raise the sides in courses over the anvil horn with the raising hammer, turning the work. Anneal to a dull red and quench whenever it stiffens.
Mga materyales para sa hakbang na ito:
Lapad na Tanso1 piraso
Tubig10 litroMga kailangang kasangkapan:
Gunting na pangyero
Martilyong pang-angat
Kahoy na Pamukpok
Palihan
Sulô ng Propano
Timbang pampatigas
Guwantes na Matibay sa Init2
2
Planish and trim
Planish and trim
Planish the pan smooth with light overlapping blows, trim the rim level and roll it slightly outward.
Mga kailangang kasangkapan:
Martilyong pang-angat
Palihan
Gunting na pangyero3
3
Handle
Handle
Forge a flat-ended handle from wrought iron rod, drill it and the pan wall, and rivet it on with copper rivets.
Mga materyales para sa hakbang na ito:
Baras ng pinandayang bakal0.3 m
Remaste na tanso3 piraso
Uling1 as requiredMga kailangang kasangkapan:
Pandayan ng panday
Martilyong pahalang ang tulis
Sipit ng panday
Barenang de-kamay4
4
Tin the inside
Tin the inside
Scour the inside bright with sandstone. Heat the pan and rub it with sal ammoniac until perfectly clean. Put tin and a little pounded rosin in, keep it hot enough to melt the tin, and spread it thinly over the whole inside with a pad of tow. Work outdoors: the sal ammoniac fumes.
Mga materyales para sa hakbang na ito:
Tinggang lingote10 g
Ammonium chloride (NH₄Cl)10 g
Dagta ng pino (rosin)5 g
Maikling hibla ng lino1 pirasoMga kailangang kasangkapan:
Sulô ng Propano
Guwantes na Matibay sa Init
Maskara Laban sa Alikabok5
5
How little tin
How little tin
Naglo-load ng Jupyter notebook…
Mga Materyales
9- 1 pirasoPlaceholder
- 10 litroPlaceholder
- Placeholder
- 3 pirasoPlaceholder
- 1 as requiredPlaceholder
- 10 gPlaceholder
- Placeholder
- Placeholder
- 1 pirasoPlaceholder
Mga Kinakailangang Kasangkapan
12- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
Ang blueprint na ito ay gumagawa ng
Kaugnay na Blueprint
Ang mga blueprint na ito ay nagbabahagi ng kaalaman — mga teknik, materyales, o prinsipyo
CC0 Pampublikong Domain
Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.
Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.