Yttrium: Fluoride Reduced with Calcium and Magnesium at 1000 °C, then Distilled to Sponge (Carlson, Schmidt and Spedding, US 2,950,962)
Charlie

Nilikha ni

Charlie

1. Nobyembre 2026DE
4
0
0
0
0

Yttrium: Fluoride Reduced with Calcium and Magnesium at 1000 °C, then Distilled to Sponge (Carlson, Schmidt and Spedding, US 2,950,962)

Calcium alone reduces yttrium fluoride only at 1500 °C. Adding magnesium makes a low-melting yttrium-magnesium alloy, and calcium chloride thins the slag, so the job runs at about 1000 °C. The magnesium and calcium are then boiled off in vacuum, leaving yttrium sponge. Result: yttrium sponge (yield 98-99 % in the alloy step), usable as a getter or remelted to an ingot. Source: O. N. Carlson, F. A. Schmidt and F. H. Spedding, US 2,950,962 (1960). Hot work under argon; calcium reacts with water. Picture drawn by Youblob.
Abantado
2 days

Mga Tagubilin

1

Weigh and mix the charge

Dry the calcium chloride in vacuum at about 550 °C. Mix thoroughly 2600 g of pure, fine yttrium fluoride, 2090 g of calcium chloride, 1285 g of granular calcium (about 20 % excess) and 395 g of magnesium turnings, and pack it into a zirconium crucible with a lid carrying a pressure-release valve.

Mga materyales para sa hakbang na ito:

Yttrium fluorideYttrium fluoride1 2600 g

Mga kailangang kasangkapan:

KalsyoKalsyo
MagnesiyoMagnesiyo
Calcium chlorideCalcium chloride
Bombang panghigop ng hanginBombang panghigop ng hangin
Crucible na zirconiumCrucible na zirconium
2

Reduce at about 1000 °C

Under argon (or helium) at about atmospheric pressure, set the crucible in a furnace already at 950-1050 °C and keep heating for about half an hour; the reaction gives off little heat. An yttrium-magnesium-calcium alloy forms under a calcium fluoride-calcium chloride slag.

Mga kailangang kasangkapan:

Crucible na zirconiumCrucible na zirconium
Pugon na may cruciblePugon na may crucible
ArgonArgon
3

Separate alloy and slag

Take the retort out and tilt it about 15° from horizontal so the slag and alloy freeze in thin layers along the side wall, then break them apart. The alloy is brittle (typically 19 % magnesium, 7-8 % calcium). Crush it to pieces of about 1/2 in.

Mga kailangang kasangkapan:

Crucible na zirconiumCrucible na zirconium
Almires at PanghaloAlmires at Panghalo
4

Boil off magnesium and calcium in vacuum

Pack the pieces in a crucible of the same metal set in a graphite heater inside a quartz tube. Pump down to about 1 micron or less and heat by induction to about 800 °C, then more slowly to 1100 °C (about three hours). The alloy does not melt; magnesium and calcium distil away (about 27 % weight loss), leaving porous yttrium sponge.

Mga kailangang kasangkapan:

Crucible na zirconiumCrucible na zirconium
Graphite na crucibleGraphite na crucible
Tubong fused quartzTubong fused quartz
Bombang panghigop ng hanginBombang panghigop ng hangin
Induction furnaceInduction furnace
5

Remelt to an ingot (optional)

Use the sponge as it is (for example as a getter in vacuum tubes), or remelt it in a consumable arc furnace under helium or vacuum to get a solid ingot.

Mga kailangang kasangkapan:

Pugon na de-kuryenteng arkoPugon na de-kuryenteng arko

Mga Materyales

1

Mga Kinakailangang Kasangkapan

12

Ang blueprint na ito ay gumagawa ng

CC0 Pampublikong Domain

Ang blueprint na ito ay inilabas sa ilalim ng CC0. Malaya kang kumopya, magbago, mamahagi, at gumamit nang walang pahintulot.

Suportahan ang Maker sa pamamagitan ng pagbili ng mga produkto sa kanilang Blueprint Komisyon ng Maker itinakda ng mga Vendor, o lumikha ng bagong bersyon ng Blueprint na ito at isama bilang koneksyon sa iyong Blueprint upang ibahagi ang kita.

Talakayan

(0)

Mag-login upang sumali sa talakayan

Naglo-load ng mga komento...