Metal Electrode Arc Welding

Carbon arc welding needs two hands: one holds the arc, the other feeds filler wire into the pool. The improvement is almost embarrassingly simple once stated — make the electrode out of the filler. Now the rod that carries the arc also melts into the joint, one hand does the work of two, and the metal crosses the arc as fine droplets rather than being pushed in cold from the side.

Charles L. Coffin patented it as US 428,459, “Process of Welding Metals Electrically”, granted 20 May 1890. It is the first verifiable patent for metal-electrode arc welding, and it describes the transfer directly: metal is carried across the arc from the electrode to the work.

Priority is not the same as patent, and this blueprint says so. Nikolay Gavrilovich Slavyanov demonstrated a consumable metal electrode at Perm in 1888, two years earlier, casting metal into a mould with the arc. No citable patent number for that work could be verified from any source, so the blueprint is built on the document that exists and credits the man who was first. Function is the payload; attribution is metadata, and both are reported honestly.

The experiment below is a measurement, not a weld: you will weigh the electrode before and after and prove that the missing mass is now in the joint.

اعلیٰ
45 minutes

ہدایات

1

Read the safety step first

Read step 12 before striking anything. Arc ultraviolet injures eyes faster than you can decide to look away.

درکار اوزار:

Notebook and PencilNotebook and Pencil
2

Weigh the electrode to 0.01 g

Weigh a single bare steel electrode. Record the mass. This number is the whole experiment.

اس مرحلے کے لیے مواد:

Metal Electrode SetMetal Electrode Set1 ٹکڑا

درکار اوزار:

Digital Scale (0.01g)Digital Scale (0.01g)
3

Weigh the test coupon

Clean a steel flat bar coupon with 220 grit until bright, then weigh it. Rust and scale would falsify the mass balance.

اس مرحلے کے لیے مواد:

Mild Steel Flat BarMild Steel Flat Bar1 ٹکڑا
Sandpaper (220 Grit)Sandpaper (220 Grit)1 شیٹ

درکار اوزار:

Digital Scale (0.01g)Digital Scale (0.01g)
4

Set the work on firebrick and clamp the return

Lay the coupon on firebrick. Clamp the return lead to the coupon itself, not to the bench.

اس مرحلے کے لیے مواد:

Mild Steel Flat BarMild Steel Flat Bar1 ٹکڑا
FirebricksFirebricks2 ٹکڑے

درکار اوزار:

C-ClampC-Clamp
5

Gear up and check the helmet

Auto-darkening helmet, leather gloves, covered arms. Test the lens before striking.

درکار اوزار:

Auto-Darkening Welding HelmetAuto-Darkening Welding Helmet
Leather GlovesLeather Gloves
6

Run a single short bead

Strike by scratching, hold a short arc, and run one 40 mm bead along the coupon at a steady pace. Stop. Do not chase a second pass.

اس مرحلے کے لیے مواد:

Metal Electrode SetMetal Electrode Set1 ٹکڑا
Mild Steel Flat BarMild Steel Flat Bar1 ٹکڑا

درکار اوزار:

Auto-Darkening Welding HelmetAuto-Darkening Welding Helmet
7

Let everything cool, then re-weigh both

Cool to room temperature. Weigh the remaining electrode stub and the coupon again. Record both.

درکار اوزار:

Digital Scale (0.01g)Digital Scale (0.01g)
8

Do the mass balance

Electrode lost, coupon gained. Compare the two numbers. The coupon gains less than the electrode loses — the difference left as spatter and oxide.

اس مرحلے کے لیے مواد:

Graph PaperGraph Paper1 شیٹ

درکار اوزار:

Notebook and PencilNotebook and Pencil
9

Calculate the deposition efficiency

Divide the coupon's gain by the electrode's loss and multiply by 100. That percentage is deposition efficiency, a number every welding consumable is still sold on.

اس مرحلے کے لیے مواد:

Graph PaperGraph Paper1 شیٹ

درکار اوزار:

Notebook and PencilNotebook and Pencil
10

Measure the bead and find the spatter

Measure bead width and length with the caliper. Look at the plate around the bead: the scattered beads of frozen metal are the missing mass.

درکار اوزار:

Vernier CaliperVernier Caliper
Magnifying GlassMagnifying Glass
11

Record what a bare electrode cannot do

Note the bead's appearance: porous, dark, irregular. Nothing protected the pool from the air. Kjellberg fixes this seventeen years later.

اس مرحلے کے لیے مواد:

Notebook and PencilNotebook and Pencil1 ٹکڑا
12

Safety awareness — arc eye and fume

An electric arc emits ultraviolet light strong enough to burn the cornea in seconds. The injury is called photokeratitis, or “arc eye”. It is not felt at the time — the pain arrives six to twelve hours later, typically in the middle of the night, and feels like sand under the eyelids. It normally heals in a day or two, but repeated exposure is cumulative.

Nobody in the room may look at an arc unshielded, including bystanders. Ordinary safety glasses do not protect against it and neither does a quick glance. Use an auto-darkening helmet, screen the work so passers-by cannot see it, and warn anyone nearby before striking. The same ultraviolet burns exposed skin like strong sunburn, so cover arms and neck.

Fume. Arc welding steel makes a metal-oxide smoke that should never be breathed. Ventilate, keep your head out of the plume, and use plain mild steel only — galvanised coatings release zinc oxide and cause metal fume fever.

Hot metal has no colour. Steel stops glowing at around 500 °C and is still hot enough to cause an immediate deep burn. Assume anything you have welded is hot until measured otherwise.

درکار اوزار:

Auto-Darkening Welding HelmetAuto-Darkening Welding Helmet
Leather GlovesLeather Gloves
Infrared ThermometerInfrared Thermometer
13

History & Context

US 428,459, “Process of Welding Metals Electrically”, Charles L. Coffin, granted 20 May 1890. Coffin, of Detroit, is the first person to hold a verifiable American patent for using a metal electrode that is itself consumed into the joint.

Slavyanov came first and this blueprint says so. Nikolay Gavrilovich Slavyanov (1854-1897), chief of the Perm cannon works, demonstrated arc welding with a consumable metal electrode in 1888 and used it to repair castings and to cast metal directly in a mould under the arc. He also introduced a molten-slag blanket over the pool — an idea that reappears in 1936 as submerged arc welding. What is missing is a patent number that any source could confirm. The honest position is that Slavyanov was first to the technique and Coffin was first to the document, and the blueprint prints both.

Why metal transfer changes everything. With a carbon electrode the filler arrives cold and unmixed. With a consumable electrode the metal crosses as droplets that have passed through the arc's own plasma, arriving superheated and alloyed. That is why consumable-electrode processes penetrate deeper at the same current, and why every dominant welding process today — stick, MIG, flux-cored, submerged arc — is a consumable electrode process. TIG, in 1942, is the deliberate exception.

What Coffin's bare rod could not solve. A bare electrode leaves the pool naked in the atmosphere. Nitrogen and oxygen dissolve into it, giving porosity, brittleness and a weld with perhaps half the parent metal's ductility. Almost every welding process developed after Coffin is, one way or another, an answer to that single problem.

مواد

6

درکار اوزار

8

CC0 پبلک ڈومین

یہ بلیو پرنٹ CC0 کے تحت جاری کیا گیا ہے۔ آپ اجازت لیے بغیر اس کام کو نقل، ترمیم، تقسیم اور کسی بھی مقصد کے لیے استعمال کرنے کے لیے آزاد ہیں۔

میکر کی حمایت کریں ان کے بلیو پرنٹ کے ذریعے پروڈکٹس خرید کر جہاں وہ میکر کمیشن وینڈرز کی طرف سے مقرر، کماتے ہیں، یا اس بلیو پرنٹ کی نئی تکرار بنائیں اور آمدنی شیئر کرنے کے لیے اسے اپنے بلیو پرنٹ میں کنکشن کے طور پر شامل کریں۔

بحث

(0)

لاگ ان بحث میں شامل ہونے کے لیے

تبصرے لوڈ ہو رہے ہیں...