A small one-handed axe forged from a 7/8 × 2-inch bar of good tool steel, best made by two people; a 6¾-inch bar gives two heads. The eye, about 9/16 × 1½ inches, is punched at a yellow heat with an eye punch and opened with drifts, the blade drawn out to a 3-inch edge and the head cut to length. The axe is annealed in lime or ashes, ground and buffed, then hardened from the hardening heat in tepid water and tempered by two hot iron bars laid on either side at the centre: dark purple for the blade, blue for the head.
اعلیٰ
4–6 hours

ہدایات

1

Mark and punch the eye

Mark the stock with chisel and centre punch. At a yellow heat, punch the eye with the narrow edge of the punch toward the blade; lift the punch after each blow to check it runs straight and to let it cool; a little fine coal in the hole stops it sticking. Punch nearly through, then finish from the other side.

اس مرحلے کے لیے مواد:

چپٹی ٹول اسٹیل کی سلاخچپٹی ٹول اسٹیل کی سلاخ1 ٹکڑا

درکار اوزار:

مرکزی سنبہمرکزی سنبہ
لوہار کی بھٹیلوہار کی بھٹی
نہائینہائی
گرم سوراخ کنگرم سوراخ کن
بڑا ہتھوڑابڑا ہتھوڑا
لوہار کی سنڈاسیلوہار کی سنڈاسی
2

Drift and draw out

Drive in a tool-steel drift, hammer the bulges down to the bar's size and smooth with a flatter; take the drift out before each reheat. Use two drifts, the first 3/8 inch narrower. Draw out the blade, driving the drift back in as the eye stretches so no cold shut forms.

درکار اوزار:

سوراخ بڑا کرنے والا اوزارسوراخ بڑا کرنے والا اوزار
ہموار کرنے کا اوزارہموار کرنے کا اوزار
اٹھاؤ گراؤ ہتھوڑااٹھاؤ گراؤ ہتھوڑا
3

Shape and trim

Shape the blade with a heavy hammer and flatter and form its edge. Cut the head from the bar, draw it to size, cut it to length, then trim the blade to shape.

درکار اوزار:

کٹائی کا ہتھوڑاکٹائی کا ہتھوڑا
ہموار کرنے کا اوزارہموار کرنے کا اوزار
گرم چھینیگرم چھینی
4

Anneal and grind

Heat to a full red and anneal in lime or ashes. When cold, grind on an emery wheel and finish on a buffing wheel.

درکار اوزار:

لوہار کی بھٹیلوہار کی بھٹی
میز کی گھسائی مشینمیز کی گھسائی مشین
5

Harden and temper

Heat very slowly to the hardening heat and cool in tepid water. Draw the temper with two hot iron bars laid on either side at the centre; when the blade is dark purple and the head blue, cool quickly in water.

درکار اوزار:

لوہار کی بھٹیلوہار کی بھٹی
آب دینے کی بالٹیآب دینے کی بالٹی
لوہار کی سنڈاسیلوہار کی سنڈاسی
6

Handle

Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.

اس مرحلے کے لیے مواد:

دستے کے لیے سخت لکڑیدستے کے لیے سخت لکڑی1 ٹکڑا
سخت لکڑی کا پھاناسخت لکڑی کا پھانا1 ٹکڑا
السی کا تیلالسی کا تیل10 ملی لیٹر

درکار اوزار:

دو دستوں والا رندہدو دستوں والا رندہ
دو آدمیوں کی عرضی آریدو آدمیوں کی عرضی آری
میز کا شکنجہمیز کا شکنجہ

مواد

4

درکار اوزار

16

یہ بلوپرنٹ بناتا ہے

متعلقہ بلیو پرنٹ

یہ بلیو پرنٹ علم بانٹتے ہیں — تکنیک، مواد یا اصول

CC0 پبلک ڈومین

یہ بلیو پرنٹ CC0 کے تحت جاری کیا گیا ہے۔ آپ اجازت لیے بغیر اس کام کو نقل، ترمیم، تقسیم اور کسی بھی مقصد کے لیے استعمال کرنے کے لیے آزاد ہیں۔

میکر کی حمایت کریں ان کے بلیو پرنٹ کے ذریعے پروڈکٹس خرید کر جہاں وہ میکر کمیشن وینڈرز کی طرف سے مقرر، کماتے ہیں، یا اس بلیو پرنٹ کی نئی تکرار بنائیں اور آمدنی شیئر کرنے کے لیے اسے اپنے بلیو پرنٹ میں کنکشن کے طور پر شامل کریں۔

بحث

(0)

لاگ ان بحث میں شامل ہونے کے لیے

تبصرے لوڈ ہو رہے ہیں...