Glass Tube: Drawn by Two Glassmakers Walking Apart (Pellatt, 1849)
How glass tube was made by hand: a blown gather of glass is welded at one end to a second rod, and two workers walk away from each other while turning, stretching the hot glass into a tube up to 60 or 70 feet long. Because the whole bubble stretches evenly, the bore and the wall stay in the same proportion all along the tube.
Result: long glass tube of nearly even bore, cut into lengths when cold. Solid cane is made the same way without blowing.
Source: Apsley Pellatt, Curiosities of Glass Making (1849), pp. 106-108. Unknown: the glass batch and the gather's size. Picture: the book's figures.
ماہر
Unknown
ہدایات
1
1
Gather and blow the ball
Gather and blow the ball
Gather a solid ball of flint glass on the end of the blowing iron and blow it out a little, so it is hollow. When it has partly cooled, use it as a core for one or more further gatherings until there is enough glass. For flat-bore thermometer tube, flatten the first ball on the marver with an iron or wooden battledore before the later gatherings. Ours: lead crystal. Not given: the amount of glass.
اس مرحلے کے لیے مواد:
سیسے والا بلور1 flint glassدرکار اوزار:
1100 درجہ سینٹی گریڈ تک پہنچ سکنے والی شیشے کی بھٹی
شیشہ پھونکنے کی نلی
مارور (شیشہ لپیٹنے کا پاٹ)2
2
Swing it long and fix the post
Swing it long and fix the post
Lengthen the ball by swinging it, and chill its far end by dipping it in cold water. A second worker makes a disc of hot glass on a rod, the 'post', and holds it upright near the ground. The chief worker climbs onto a chair and drops the hot ball onto the post, where it welds on.
درکار اوزار:
پانی
پونٹل چھڑ3
3
Walk apart and draw
Walk apart and draw
The chief worker steps down and the two walk away from each other, both turning their rods all the time. At first the hot glass sags between them in a curve; fan the parts that are thicker to cool them, so it stretches evenly. Draw it to the length wanted, up to 60 or 70 feet; as it cools it stops turning and pulls nearly straight. Except at the ends, it has nearly one bore, diameter and wall thickness. Ours: a wooden paddle for fanning (Pellatt: a boy's hat).
درکار اوزار:
شیشہ پھونکنے کی نلی
پونٹل چھڑ
لکڑی کا چپو4
4
Lay down and cut
Lay down and cut
Lay the tube across the wooden rungs of a ladder to cool. Cut it into lengths by touching it with a cold iron or nicking it with a steel file.
درکار اوزار:
لکڑی کی سیڑھی
دھات کی ریتیمواد
1- 1 flint glassپلیس ہولڈر
درکار اوزار
8- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
منسلک بلیو پرنٹ مواد
یہ بلوپرنٹ بناتا ہے
CC0 پبلک ڈومین
یہ بلیو پرنٹ CC0 کے تحت جاری کیا گیا ہے۔ آپ اجازت لیے بغیر اس کام کو نقل، ترمیم، تقسیم اور کسی بھی مقصد کے لیے استعمال کرنے کے لیے آزاد ہیں۔
میکر کی حمایت کریں ان کے بلیو پرنٹ کے ذریعے پروڈکٹس خرید کر جہاں وہ میکر کمیشن وینڈرز کی طرف سے مقرر، کماتے ہیں، یا اس بلیو پرنٹ کی نئی تکرار بنائیں اور آمدنی شیئر کرنے کے لیے اسے اپنے بلیو پرنٹ میں کنکشن کے طور پر شامل کریں۔