PETG Pellets: Dimethyl Terephthalate with Ethylene Glycol and CHDM
PETG is PET in which part of the ethylene glycol is replaced by CHDM, which keeps the plastic clear and amorphous. Eastman's patent US 7,026,027 describes PETG 6763 as terephthalate with about 69 mol % ethylene glycol and 31 mol % CHDM, but gives no recipe for it. This blueprint is our own combination: that composition, made by the same patent's pilot-plant process (Example 12, written for a CHDM/neopentyl glycol copolyester), with ethylene glycol in place of neopentyl glycol as in Kibler's 1959 Eastman patent. The charge weights are our arithmetic.
The picture: our diagram.
اعلیٰ
About 5 hours
ہدایات
1
1
Charge the reactor
Charge the reactor
Our charge for 31 mol % CHDM: 10.669 kg dimethyl terephthalate (54.9 mol, as in the patent's example), 2.456 kg CHDM (31 % of those moles) and 4.058 kg ethylene glycol, so the glycols total 1.5 times the ester moles as in the example. Add 53.4 g of catalyst solution (15 g titanium isopropoxide in 250 ml n-butanol). The patent's reactor held 18 gallons and had spiral agitators and a distillation column.
اس مرحلے کے لیے مواد:
ڈائی میتھائل ٹیریفتھیلیٹ10.669 کلوگرام
1,4-سائیکلوہیکسین ڈائی میتھانول2.456 کلوگرام
ایتھیلین گلائکول4.058 کلوگرامدرکار اوزار:
ٹائٹینیم آئسوپروپوکسائیڈ
این-بیوٹانول
پلڑوں والی ترازو
جیکٹ والا پولیمرائزیشن ری ایکٹر
جزوی کشید کی بھٹی
کیمیائی چھینٹوں سے بچاؤ کا چشمہ2
2
Ester interchange at 200 °C
Ester interchange at 200 °C
Stir (forward 50 minutes, then reverse 10), heat to 200 °C and hold 2 hours. Methanol distils off through the column.
درکار اوزار:
جیکٹ والا پولیمرائزیشن ری ایکٹر
جزوی کشید کی بھٹی
پیمائش والا تھرموکپل3
3
260 °C, then 280 °C
260 °C, then 280 °C
Raise to 260 °C for 30 minutes and weigh the distillate, then raise to 280 °C and weigh it again. The surplus ethylene glycol is driven off; Kibler found the CHDM stays in the polymer.
درکار اوزار:
جیکٹ والا پولیمرائزیشن ری ایکٹر
پیمائش والا تھرموکپل
پلڑوں والی ترازو4
4
Polymerise under vacuum
Polymerise under vacuum
Switch the agitator direction every 6 minutes and pull vacuum at 13 Torr a minute down to 0.5 Torr. Hold full vacuum for 45 minutes at 25 rpm.
درکار اوزار:
جیکٹ والا پولیمرائزیشن ری ایکٹر
خلائی پمپ
خلا پیما
کولڈ ٹریپ5
5
Extrude and chop into pellets
Extrude and chop into pellets
Let nitrogen in, extrude the polymer at once and chop it into pellets. Check the composition: in the patent's example the polymer kept slightly less CHDM than was charged (38.1 % for 40.7 %).
درکار اوزار:
نائٹروجن گیس سلنڈر
پیلیٹائزر
حرارت روک دستانےمواد
3- 10.669 کلوگرامپلیس ہولڈر
- 2.456 کلوگرامپلیس ہولڈر
- 4.058 کلوگرامپلیس ہولڈر
درکار اوزار
13- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- 1 vendor sell this, none ship to you yetپلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
یہ بلوپرنٹ بناتا ہے
متعلقہ بلیو پرنٹ
یہ بلیو پرنٹ علم بانٹتے ہیں — تکنیک، مواد یا اصول

خطرناک
1,4-Cyclohexanedimethanol: Dimethyl Terephthalate Hydrogenated over Palladium, then Copper Chromite
Charlie کی طرف سے
صنعتی
3
0
0
0
0
0

Dimethyl Terephthalate: Terephthalic Acid and Methanol Sprayed through a Hot Tube
Charlie کی طرف سے
صنعتی
3
0
0
0
0
0

خطرناک
Ethylene Glycol by Hydration of Ethylene Oxide
Charlie کی طرف سے
صنعتی
5
0
0
0
0
0
CC0 پبلک ڈومین
یہ بلیو پرنٹ CC0 کے تحت جاری کیا گیا ہے۔ آپ اجازت لیے بغیر اس کام کو نقل، ترمیم، تقسیم اور کسی بھی مقصد کے لیے استعمال کرنے کے لیے آزاد ہیں۔
میکر کی حمایت کریں ان کے بلیو پرنٹ کے ذریعے پروڈکٹس خرید کر جہاں وہ میکر کمیشن وینڈرز کی طرف سے مقرر، کماتے ہیں، یا اس بلیو پرنٹ کی نئی تکرار بنائیں اور آمدنی شیئر کرنے کے لیے اسے اپنے بلیو پرنٹ میں کنکشن کے طور پر شامل کریں۔