Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)
The file for sharpening saw teeth as Sheffield made it by hand: a three-square (triangular) bar of cast steel, not tapering, forged in a V-shaped boss, its teeth cut one by one with a chisel and hammer, then hardened under a coat of animal carbon and salt and quenched in cold spring water.
Ure says saw files in particular should be hardened with the carbon mixture, so they will cut iron and steel.
Not given: sizes and teeth per inch.
Source: A. Ure, Dictionary of Arts, Manufactures, and Mines (1839), File. Picture: our drawing.
اعلیٰ
Unknown
ہدایات
1
1
Forge the blank
Forge the blank
Draw cast steel out square at the forge, then lay it with one angle down in a boss whose recess has two sides meeting at an angle, so the hammer forms one side and the boss the other two. Keep it the same size along its length (saw files are not tapered).
اس مرحلے کے لیے مواد:
کٹھالی فولاد1 cast steel bar
نامعلوم پیمائش1 ٹکڑادرکار اوزار:
لوہار کی بھٹی
لوہار کی چمٹی
نچلا سواج
ہتھوڑا
بڑا ہتھوڑا2
2
Cut the teeth
Cut the teeth
On an anvil with a flat, even face, hold the file down with a leather strap over each end, the workman's feet in the straps like stirrups. Cut the teeth with a chisel a little broader than the file, sharpened to about 20 degrees, struck with a hammer of 1 to 6 lb. For single cut, run a fine file lightly over the teeth to take off the roughness; for double cut, cut a second set nearly at right angles to the first.
درکار اوزار:
فولادی اہرن
چمڑے کا تسمہ
ٹھنڈی چھینی
ہتھوڑا
دھات کی ریتی3
3
Cut the other sides
Cut the other sides
To cut the next side, lay the file in a piece of lead-tin alloy with an angular groove, so the teeth already cut are not spoiled on the anvil.
درکار اوزار:
ٹن-سیسے کا ٹانکہ
فولادی اہرن
ٹھنڈی چھینی
ہتھوڑا4
4
Coat for hardening
Coat for hardening
Distil shoemakers' and curriers' leather refuse in an iron still and powder the bright coal left. Grind about equal parts by bulk of this carbon and salt to the consistence of cream with water and cover the file with it.
درکار اوزار:
لوہے کا قرع
نمک
پانی5
5
Harden
Harden
Hold the file by the tang in a fire of very small cokes, drawing it out often, until it is an even cherry red from tang to point. Plunge it straight down, quickly, into clear spring water as cold as possible.
درکار اوزار:
لوہار کی بھٹی
دھات کاری کا کوک
لوہار کی چمٹی
پانی6
6
Clean and oil
Clean and oil
Brush the file with water and powdered cokes until clean and metallic, wash it in two or three waters to take off all the salt, dip it in lime-water, dry it quickly before the fire and oil it while warm with olive oil containing a little oil of turpentine.
درکار اوزار:
دھات کاری کا کوک
پانی
چونے کا پانی
زیتون کا تیل
تارپینمواد
2- 1 cast steel barپلیس ہولڈر
- 1 ٹکڑاپلیس ہولڈر
درکار اوزار
17- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
یہ بلوپرنٹ بناتا ہے
CC0 پبلک ڈومین
یہ بلیو پرنٹ CC0 کے تحت جاری کیا گیا ہے۔ آپ اجازت لیے بغیر اس کام کو نقل، ترمیم، تقسیم اور کسی بھی مقصد کے لیے استعمال کرنے کے لیے آزاد ہیں۔
میکر کی حمایت کریں ان کے بلیو پرنٹ کے ذریعے پروڈکٹس خرید کر جہاں وہ میکر کمیشن وینڈرز کی طرف سے مقرر، کماتے ہیں، یا اس بلیو پرنٹ کی نئی تکرار بنائیں اور آمدنی شیئر کرنے کے لیے اسے اپنے بلیو پرنٹ میں کنکشن کے طور پر شامل کریں۔