Strontium Ferrite Disc Magnet, Sintered 4 Hours at 1200 °C (Went, Philips 1956, Ex. 34)
A strontium ferrite magnet made exactly like Went's barium ferrite of Example 34, with strontium carbonate in place of barium carbonate: 29.5 g of it to 191.7 g iron oxide, milled, fired, milled again, pressed and sintered for 4 hours. This iteration sinters at 1200 °C, where his rod held 1,340 gauss with a coercive force of 3,900 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 34. They pressed rods; the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
اعلیٰ
2 days
ہدایات
1
1
Weigh strontium carbonate and iron oxide
Weigh strontium carbonate and iron oxide
Weigh 29.5 g of strontium carbonate and 191.7 g of ferric oxide, Fe2O3. The patent makes this second mixture "in exactly the same manner" as the barium one.
اس مرحلے کے لیے مواد:
اسٹرونشیم کاربونیٹ29.5 گرام
فیرک آکسائیڈ191.7 گرامدرکار اوزار:
پلڑوں والی ترازو
ربڑ کے دستانے
P100 سانس محافظ2
2
Mill with ethanol for 4 hours
Mill with ethanol for 4 hours
Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.
درکار اوزار:
لوہے کی بال مل
ایتھینول - تجربہ گاہ درجہ، 95 %
سُکھانے کا تنور3
3
Presinter at 1000 °C for 4 hours
Presinter at 1000 °C for 4 hours
Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.
درکار اوزار:
مفل بھٹی
ڈھکن سمیت کروسیبل (چینی مٹی)
کٹھالی کی چمٹی
حرارت روک دستانے4
4
Mill again for 4 hours
Mill again for 4 hours
Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.
درکار اوزار:
لوہے کی بال مل
ایتھینول - تجربہ گاہ درجہ، 95 %
سُکھانے کا تنور
P100 سانس محافظ5
5
Press discs at 1.5 tons per cm²
Press discs at 1.5 tons per cm²
Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).
درکار اوزار:
ہائیڈرولک پریس
ڈسک دبانے کا سانچا6
6
Sinter 4 hours at 1200 °C
Sinter 4 hours at 1200 °C
Sinter the discs for 4 hours at 1200 °C in oxygen or in air. The patent's strontium rod at 1200 °C: 1,340 gauss and 3,900 oersted.
درکار اوزار:
مفل بھٹی
کٹھالی کی چمٹی
حرارت روک دستانے7
7
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
درکار اوزار:
برقی مقناطیس
قطب نمامواد
2- 29.5 گرامپلیس ہولڈر
- 191.7 گرامپلیس ہولڈر
درکار اوزار
14- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
یہ بلوپرنٹ بناتا ہے
متعلقہ بلیو پرنٹ
یہ بلیو پرنٹ علم بانٹتے ہیں — تکنیک، مواد یا اصول

Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)
Charlie کی طرف سے
صنعتی
11
0
0
0
0
0

Strontium Carbonate: Powdered Celestine Boiled with Soda Solution (Thorpe 1912)
Charlie کی طرف سے
صنعتی
14
0
0
0
0
0

خطرناک
Ferrite Toroid Core: Nickel-Zinc Ferrite Sintered at 1300 °C in Oxygen (Snoek)
Charlie کی طرف سے
صنعتی
17
0
0
0
0
0

Ferric Oxide: Hydroxide Precipitated from Ferric Chloride with Ammonia, Then Heated
Charlie کی طرف سے
غیر نامیاتی
12
0
0
0
0
0
CC0 پبلک ڈومین
یہ بلیو پرنٹ CC0 کے تحت جاری کیا گیا ہے۔ آپ اجازت لیے بغیر اس کام کو نقل، ترمیم، تقسیم اور کسی بھی مقصد کے لیے استعمال کرنے کے لیے آزاد ہیں۔
میکر کی حمایت کریں ان کے بلیو پرنٹ کے ذریعے پروڈکٹس خرید کر جہاں وہ میکر کمیشن وینڈرز کی طرف سے مقرر، کماتے ہیں، یا اس بلیو پرنٹ کی نئی تکرار بنائیں اور آمدنی شیئر کرنے کے لیے اسے اپنے بلیو پرنٹ میں کنکشن کے طور پر شامل کریں۔