A 6-inch silver teaspoon forged out of a small bar of silver, the way a blacksmith forges iron. Arthur Payne called it the hardest of his five spoon methods, but the cheapest, because almost no silver is wasted.
Source: A. F. Payne, Art Metalwork with Inexpensive Equipment (1914), pp. 184–186; annealing from his chapter XI. Cutting the bar from sheet is ours. Picture: Payne's Fig. 158, teaspoons forged this way.
اعلیٰ
1 day
ہدایات
1
1
Cut the silver bar
Cut the silver bar
For a teaspoon 6 in long you need a piece of sterling silver 4 in long, ½ in wide and ⅛ in thick. Mark it out and saw it from sheet of that thickness (cutting from sheet is ours).
اس مرحلے کے لیے مواد:
اسٹرلنگ چاندی کی چادر1 piece 4 × ½ × ⅛ inدرکار اوزار:
خط کھینچنے والی سوئی
جوہری کی آری2
2
Forge out the bowl
Forge out the bowl
Heat the bar until it is almost red-hot, hold it in tongs and forge the bowl out on the anvil. Silver forges more easily when it is nearly red, but never hammer it while it is red-hot: it will crack.
درکار اوزار:
بنسن برنر
چمٹا
نہائی
ہتھوڑا3
3
Work bowl, then shank and handle
Work bowl, then shank and handle
Hammer the bowl until it is hard, then the shank and handle, so the whole spoon is hard before you anneal it again. That saves time.
درکار اوزار:
نہائی
ہتھوڑا4
4
Anneal and repeat
Anneal and repeat
To soften it, heat it to a dull red and plunge it into water, or let it cool. Then go on forging until the spoon is roughly to shape.
اس مرحلے کے لیے مواد:
پانی1 as requiredدرکار اوزار:
بنسن برنر
چمٹا
شیشے کا برتن5
5
Trim with shears and file
Trim with shears and file
Trim the outline with the shears and file the edges smooth.
درکار اوزار:
بھاری دھاتی قینچی
ریتیاں (ہاتھ کی ریتی)6
6
Polish out the file marks
Polish out the file marks
Rub out all the scratches and file marks with emery cloth.
درکار اوزار:
سنبادہ کپڑا7
7
Anneal to even the fire scale
Anneal to even the fire scale
Anneal the spoon thoroughly once more. Heated silver grows a thin white skin, the fire scale, and this brings it back over the spots where filing and polishing took it off, so the colour is even.
اس مرحلے کے لیے مواد:
پانی1 as requiredدرکار اوزار:
بنسن برنر
چمٹا
شیشے کا برتن8
8
Planish with smooth hammers
Planish with smooth hammers
Planish the spoon on smooth tools with smooth, bright hammers. This makes it stiff again after the annealing.
درکار اوزار:
ہموار کرنے والی ہتھوڑی
نہائی
کھونٹا9
9
Final polish with rouge
Final polish with rouge
Polish it lightly with a soft cotton flannel and a little red rouge.
درکار اوزار:
زیور چمکانے کا کپڑا
سنار کا سرخدرکار اوزار
14- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
- پلیس ہولڈر
یہ بلوپرنٹ بناتا ہے
متعلقہ بلیو پرنٹ
یہ بلیو پرنٹ علم بانٹتے ہیں — تکنیک، مواد یا اصول
CC0 پبلک ڈومین
یہ بلیو پرنٹ CC0 کے تحت جاری کیا گیا ہے۔ آپ اجازت لیے بغیر اس کام کو نقل، ترمیم، تقسیم اور کسی بھی مقصد کے لیے استعمال کرنے کے لیے آزاد ہیں۔
میکر کی حمایت کریں ان کے بلیو پرنٹ کے ذریعے پروڈکٹس خرید کر جہاں وہ میکر کمیشن وینڈرز کی طرف سے مقرر، کماتے ہیں، یا اس بلیو پرنٹ کی نئی تکرار بنائیں اور آمدنی شیئر کرنے کے لیے اسے اپنے بلیو پرنٹ میں کنکشن کے طور پر شامل کریں۔