Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass
Charlie

Autor

Charlie

20. październik 2026DE
5
0
0
0
0

Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass

A thick acrylic block cannot be cast flawless in one pour. Tattersall (ICI, US 2,071,907, 1937) built it up in layers: pour 1/2 inch of syrup on a level glass plate, let it set for a day at room temperature, pour the next 1/2 inch on top, cover with a second glass plate, wait another day, then heat the sandwich at 80 °C. Each 1/2 inch layer shrinks to about 1/3 inch. The glass gives both faces a finished polish with no grinding. The picture: our diagram.
Średniozaawansowany
3 days

Instrukcje

1

Level the bottom plate

Set a glass plate on a ledge in a wooden frame, on a body of plaster of Paris, and level it carefully. The example sheet was 10 by 18 inches.

Potrzebne narzędzia:

SzybaSzyba
Rama drewnianaRama drewniana
Gips modelarskiGips modelarski
Poziomica 1,5 mPoziomica 1,5 m
2

Pour the first 1/2 inch

Pour room-temperature syrup 1/2 inch deep (about 1.5 litres for 10 by 18 inches; our figure). Cover against dust, but do not put the top plate on yet. Leave 24 hours at about 20 °C.

Materiały do tego kroku:

Syrop metakrylanu metyluSyrop metakrylanu metylu3 l

Potrzebne narzędzia:

Rękawice gumoweRękawice gumowe
Termometr laboratoryjnyTermometr laboratoryjny
3

Pour the next layer and cover

Pour a second 1/2 inch layer on the first. Lower the top glass plate onto it so it rests on the syrup and keeps pressing on it. Leave another 24 hours at about 20 °C. For a thicker block repeat the layers, a day apart, and put the plate on the last one.

Potrzebne narzędzia:

SzybaSzyba
4

Heat at 80 °C

Take the glass sandwich out of the frame and heat it for three hours at 80 °C to finish the polymerisation.

Potrzebne narzędzia:

Piec do suszeniaPiec do suszenia
Termometr laboratoryjnyTermometr laboratoryjny
Rękawice żaroodporneRękawice żaroodporne
5

Spring off the glass

Spring the glass plates off the block with a knife blade. Both faces come out smooth and polished.

Potrzebne narzędzia:

Nóż introligatorskiNóż introligatorski
Rękawice gumoweRękawice gumowe

Materiały

1

Wymagane narzędzia

9

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...