Activated Alumina: Aluminium Trihydrate Heated at 350 °C While Hot Air Carries the Steam Away (Derr, Alcoa, US 2,015,593)
Charlie

Autor

Charlie

30. październik 2026DE
0
0
0
0
0

Activated Alumina: Aluminium Trihydrate Heated at 350 °C While Hot Air Carries the Steam Away (Derr, Alcoa, US 2,015,593)

Heating aluminium trihydrate drives out its water and leaves a porous alumina that soaks up moisture. Alcoa's Derr found it works much better when the steam is carried away at once, by a stream of hot air or by a vacuum, instead of lingering in the bed. Result: activated alumina that takes up 14 % of its weight in water from air (8 % made the old way), up to 16 % if washed first in 3 % sulphuric acid. Source: Derr, US 2,015,593 (Alcoa, 1935). Not given: times, bed depth, air rate, amounts. Picture drawn by Youblob.
Średniozaawansowany
1 day

Instrukcje

1

Wash the trihydrate in 3 % sulphuric acid

Before heating, wash the aluminium trihydrate in water containing about 3 % by weight of sulphuric acid. Derr calls this very desirable but not essential: it raises the capacity by about 1-2 %. Ours: stir in a beaker.

Materiały do tego kroku:

Wodorotlenek glinuWodorotlenek glinu1 as required

Potrzebne narzędzia:

Rozcieńczony kwas siarkowyRozcieńczony kwas siarkowy
WodaWoda
Zlewka borokrzemowaZlewka borokrzemowa
Bagietka szklanaBagietka szklana
2

Lay it in beds in a chamber

Put the material in beds or layers in a chamber that gas can be drawn through. Ours: a tube furnace.

Potrzebne narzędzia:

Piec rurowyPiec rurowy
3

Draw air at 350 °C through the bed

Draw air (or combustion gas) heated to about 350 °C through the bed and out of the chamber in a continuous flow, so the steam leaves at once. Temperature: 250-800 °C works, 350-400 °C is best; above 800 °C the alumina changes and loses capacity.

Potrzebne narzędzia:

DmuchawaDmuchawa
PirometrPirometr
4

Or heat it under a partial vacuum

Instead of hot air, close the chamber, keep a partial vacuum in it and heat above 250 °C and below 800 °C; 300-400 °C on a large scale. The steam passes quickly out of the chamber.

Potrzebne narzędzia:

Pompa próżniowaPompa próżniowa
PirometrPirometr
5

Keep it dry

The product takes up about 14 % of its weight of water from air, 16 % if acid-washed. Ours: store it in an airtight container until use.

Potrzebne narzędzia:

Hermetyczne pojemniki do przechowywaniaHermetyczne pojemniki do przechowywania

Materiały

1

Wymagane narzędzia

9

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...