Barium-Calcium Ferrite Disc Magnet: 0.09 mol BaCO3 and 0.01 mol CaCO3 (Went, Philips 1956, Ex. 19)
Charlie

Autor

Charlie

28. październik 2026DE
3
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: 0.09 mol BaCO3 and 0.01 mol CaCO3 (Went, Philips 1956, Ex. 19)

A ceramic magnet with a tenth of the barium replaced by calcium: 0.09 mol barium carbonate and 0.01 mol calcium carbonate to 0.6 mol iron oxide, made as in Example 18: milled, presintered at 1000 °C, milled again, formed and passed through a 1330 °C furnace in 10 minutes. Went's rod held 1,705 gauss with a coercive force of 1,110 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 19. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Zaawansowany
2 days

Instrukcje

1

Weigh barium carbonate, chalk and iron oxide

Weigh 17.76 g barium carbonate (0.09 mol), 1.001 g calcium carbonate (0.01 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiały do tego kroku:

Węglan baru (witheryt)Węglan baru (witheryt)17.76 g
Węglan wapnia (kreda malarska)Węglan wapnia (kreda malarska)1.001 g
Tlenek żelaza(III)Tlenek żelaza(III)95.55 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Rękawice gumoweRękawice gumowe
Półmaska P100Półmaska P100
2

Mill with alcohol 4 hours, dry at 150 °C

Grind with alcohol in a ball mill for 4 hours and dry in air at 150 °C.

Potrzebne narzędzia:

Żelazny młyn kulowyŻelazny młyn kulowy
Etanol - klasa laboratoryjna, 95 %Etanol - klasa laboratoryjna, 95 %
Piec do suszeniaPiec do suszenia
3

Presinter in air at 1000 °C for 2 hours

Fire in air at 1000 °C for 2 hours.

Potrzebne narzędzia:

Piec muflowyPiec muflowy
Tygiel z pokrywką (porcelanowy)Tygiel z pokrywką (porcelanowy)
Szczypce do tyglaSzczypce do tygla
Rękawice żaroodporneRękawice żaroodporne
4

Mill again 4 hours, dry, form

Grind again with alcohol for 4 hours and dry. Example 19 extrudes a rod; ours: press discs at 1.5 tonnes per cm², as Example 18 moulds its rod.

Potrzebne narzędzia:

Żelazny młyn kulowyŻelazny młyn kulowy
Etanol - klasa laboratoryjna, 95 %Etanol - klasa laboratoryjna, 95 %
Piec do suszeniaPiec do suszenia
Prasa hydraulicznaPrasa hydrauliczna
Matryca do prasowania krążkówMatryca do prasowania krążków
5

Pass through a 1330 °C zone in 10 minutes

Sinter at 1330 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Potrzebne narzędzia:

Piec rurowyPiec rurowy
Rękawice żaroodporneRękawice żaroodporne
6

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Potrzebne narzędzia:

ElektromagnesElektromagnes
KompasKompas

Materiały

3

Wymagane narzędzia

15

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...