Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)
Charlie

Autor

Charlie

28. październik 2026DE
0
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: 20 % Calcium, 5 Minutes at 1290 °C (Went, Philips 1956, Ex. 20)

A ceramic magnet with a fifth of the barium replaced by calcium: 0.08 mol barium carbonate, 0.02 mol calcium carbonate and 0.6 mol iron oxide, made as in Example 18 but sintered at 1290 °C for only 5 minutes. Went's rod held 1,615 gauss with a coercive force of 1,550 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 20. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Zaawansowany
2 days

Instrukcje

1

Weigh barium carbonate, chalk and iron oxide

Weigh 15.79 g barium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol) and 95.55 g ferric oxide (0.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiały do tego kroku:

Węglan baru (witheryt)Węglan baru (witheryt)15.79 g
Węglan wapnia (kreda malarska)Węglan wapnia (kreda malarska)2.002 g
Tlenek żelaza(III)Tlenek żelaza(III)95.55 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Rękawice gumoweRękawice gumowe
Półmaska P100Półmaska P100
2

Mill, presinter and mill as in Example 18

As in Example 18: grind with alcohol 4 hours, dry at 150 °C, fire in air at 1000 °C for 2 hours, grind again 4 hours and dry.

Potrzebne narzędzia:

Żelazny młyn kulowyŻelazny młyn kulowy
Etanol - klasa laboratoryjna, 95 %Etanol - klasa laboratoryjna, 95 %
Piec do suszeniaPiec do suszenia
Piec muflowyPiec muflowy
Tygiel z pokrywką (porcelanowy)Tygiel z pokrywką (porcelanowy)
Szczypce do tyglaSzczypce do tygla
3

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm², as in Example 18 (ours: discs instead of rods).

Potrzebne narzędzia:

Prasa hydraulicznaPrasa hydrauliczna
Matryca do prasowania krążkówMatryca do prasowania krążków
4

Pass through a 1290 °C zone in 5 minutes

Sinter in air at 1290 °C by passing the pieces through a 10 cm hot zone at 20 mm per minute: 5 minutes in the heat.

Potrzebne narzędzia:

Piec rurowyPiec rurowy
Rękawice żaroodporneRękawice żaroodporne
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Potrzebne narzędzia:

ElektromagnesElektromagnes
KompasKompas

Materiały

3

Wymagane narzędzia

15

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...