Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)
Charlie

Autor

Charlie

28. październik 2026DE
0
0
0
0
0

Barium-Calcium Ferrite Disc Magnet: Equal Barium and Calcium, Sintered at 1280 °C (Went, Philips 1956, Ex. 22)

A ceramic magnet with equal parts barium and calcium: 0.3 mol barium carbonate, 0.3 mol calcium carbonate and 3.1 mol iron oxide, milled 15 hours, pressed and passed through a 1280 °C furnace in 10 minutes, with no presintering. Went's rod held 1,595 gauss with a coercive force of 1,890 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 22. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Zaawansowany
2 days

Instrukcje

1

Weigh barium carbonate, chalk and iron oxide

Weigh 59.5 g barium carbonate (0.3 mol), 30.2 g calcium carbonate (0.3 mol) and 500.0 g ferric oxide (3.1 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiały do tego kroku:

Węglan baru (witheryt)Węglan baru (witheryt)59.5 g
Węglan wapnia (kreda malarska)Węglan wapnia (kreda malarska)30.2 g
Tlenek żelaza(III)Tlenek żelaza(III)500 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Rękawice gumoweRękawice gumowe
Półmaska P100Półmaska P100
2

Mill with alcohol 15 hours, dry, press

Grind with alcohol in a ball mill for 15 hours, dry, and press at 1.5 tonnes per cm² (ours: discs instead of rods). No presintering.

Potrzebne narzędzia:

Żelazny młyn kulowyŻelazny młyn kulowy
Etanol - klasa laboratoryjna, 95 %Etanol - klasa laboratoryjna, 95 %
Piec do suszeniaPiec do suszenia
Prasa hydraulicznaPrasa hydrauliczna
Matryca do prasowania krążkówMatryca do prasowania krążków
3

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Potrzebne narzędzia:

Piec rurowyPiec rurowy
Rękawice żaroodporneRękawice żaroodporne
4

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Potrzebne narzędzia:

ElektromagnesElektromagnes
KompasKompas

Materiały

3

Wymagane narzędzia

12

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...