Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)
Charlie

Autor

Charlie

28. październik 2026DE
1
0
0
0
0

Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)

A barium ferrite magnet made from natural magnetite instead of ferric oxide: barium carbonate and magnetite ground 18 hours, presintered 3 hours at 900 °C, ground again 18 hours, pressed and sintered 2 hours at 1200 °C. Went's rod held 1,450 gauss with a coercive force of 2,425 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Zaawansowany
2 days

Instrukcje

1

Weigh barium carbonate and magnetite

Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiały do tego kroku:

Węglan baru (witheryt)Węglan baru (witheryt)9.9 g
MagnetytMagnetyt46.9 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Rękawice gumoweRękawice gumowe
Półmaska P100Półmaska P100
2

Grind 18 hours in a ball mill

Grind the mixture in a ball mill for 18 hours. The patent does not say whether wet or dry.

Potrzebne narzędzia:

Żelazny młyn kulowyŻelazny młyn kulowy
Półmaska P100Półmaska P100
3

Presinter at 900 °C for 3 hours

Fire the ground mixture at 900 °C for three hours and let it cool.

Potrzebne narzędzia:

Piec muflowyPiec muflowy
Tygiel z pokrywką (porcelanowy)Tygiel z pokrywką (porcelanowy)
Szczypce do tyglaSzczypce do tygla
Rękawice żaroodporneRękawice żaroodporne
4

Grind 18 hours in a ball mill

Grind it again in a ball mill for 18 hours. The patent does not say whether wet or dry.

Potrzebne narzędzia:

Żelazny młyn kulowyŻelazny młyn kulowy
Półmaska P100Półmaska P100
5

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm² (ours: discs instead of a rod).

Potrzebne narzędzia:

Prasa hydraulicznaPrasa hydrauliczna
Matryca do prasowania krążkówMatryca do prasowania krążków
6

Sinter at 1200 °C for 2 hours

Sinter at 1200 °C for 2 hours. The patent gives no atmosphere for this example. Went's rod: 1,450 gauss, 2,425 oersted.

Potrzebne narzędzia:

Piec muflowyPiec muflowy
Szczypce do tyglaSzczypce do tygla
Rękawice żaroodporneRękawice żaroodporne
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Potrzebne narzędzia:

ElektromagnesElektromagnes
KompasKompas

Materiały

2

Wymagane narzędzia

12

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...