Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)
Charlie

Autor

Charlie

28. październik 2026DE
0
0
0
0
0

Barium Ferrite Disc Magnet: 0.5 mol BaCO3 to 3.5 mol Iron Oxide, 10 Minutes at 1330 °C (Went, Philips 1956, Ex. 4)

A barium ferrite with much more iron oxide: 0.5 mol barium carbonate to 3.5 mol, milled 15.5 hours, bound, formed and sintered 10 minutes at 1330 °C. Went's rod held 2,040 gauss with a coercive force of 2,380 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 4. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Zaawansowany
2 days

Instrukcje

1

Weigh barium carbonate and iron oxide

Weigh 99.2 g barium carbonate (0.5 mol) and 564.8 g ferric oxide (3.5 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiały do tego kroku:

Węglan baru (witheryt)Węglan baru (witheryt)99.2 g
Tlenek żelaza(III)Tlenek żelaza(III)564.8 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Rękawice gumoweRękawice gumowe
Półmaska P100Półmaska P100
2

Mill with alcohol 15.5 hours, dry and sieve

Grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

Potrzebne narzędzia:

Żelazny młyn kulowyŻelazny młyn kulowy
Etanol - klasa laboratoryjna, 95 %Etanol - klasa laboratoryjna, 95 %
Piec do suszeniaPiec do suszenia
PrzesiewaczPrzesiewacz
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

Potrzebne narzędzia:

Polialkohol winylowy w proszkuPolialkohol winylowy w proszku
Prasa hydraulicznaPrasa hydrauliczna
Matryca do prasowania krążkówMatryca do prasowania krążków
Piec do suszeniaPiec do suszenia
4

Sinter in air at 1330 °C for 10 minutes

Sinter the pieces in air at 1330 °C for 10 minutes. The patent gives no zone length or speed for this example.

Potrzebne narzędzia:

Piec rurowyPiec rurowy
Rękawice żaroodporneRękawice żaroodporne
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Potrzebne narzędzia:

ElektromagnesElektromagnes
KompasKompas

Materiały

2

Wymagane narzędzia

14

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...