Barium-Strontium Ferrite Disc Magnet: 0.21 mol BaCO3, 0.09 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 30)
Charlie

Autor

Charlie

28. październik 2026DE
1
0
0
0
0

Barium-Strontium Ferrite Disc Magnet: 0.21 mol BaCO3, 0.09 mol SrCO3, 1300 °C (Went, Philips 1956, Ex. 30)

A ceramic magnet with both barium and strontium: 0.21 mol barium carbonate and 0.09 mol strontium carbonate to 2.7 mol iron oxide, milled as in Example 28, pressed and passed through a 1300 °C furnace in 10 minutes. Went's rod held 1,245 gauss with a coercive force of 2,370 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 30. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Zaawansowany
2 days

Instrukcje

1

Weigh the carbonates and iron oxide

Weigh 41.7 g barium carbonate (0.21 mol), 13.3 g strontium carbonate (0.09 mol), 435.5 g ferric oxide (2.7 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiały do tego kroku:

Węglan baru (witheryt)Węglan baru (witheryt)41.7 g
Węglan strontuWęglan strontu13.3 g
Tlenek żelaza(III)Tlenek żelaza(III)435.5 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Rękawice gumoweRękawice gumowe
Półmaska P100Półmaska P100
2

Mill with alcohol 15 hours, dry

As in Example 28: grind the mixture with alcohol in a ball mill for 15 hours, then dry it.

Potrzebne narzędzia:

Żelazny młyn kulowyŻelazny młyn kulowy
Etanol - klasa laboratoryjna, 95 %Etanol - klasa laboratoryjna, 95 %
Piec do suszeniaPiec do suszenia
3

Press the powder

Example 28 moulds a rod without giving the pressure. Ours: press discs at 1.5 tonnes per cm², the pressure of the patent's other examples.

Potrzebne narzędzia:

Prasa hydraulicznaPrasa hydrauliczna
Matryca do prasowania krążkówMatryca do prasowania krążków
4

Pass through a 1300 °C zone in 10 minutes

Sinter in air at 1300 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Potrzebne narzędzia:

Piec rurowyPiec rurowy
Rękawice żaroodporneRękawice żaroodporne
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Potrzebne narzędzia:

ElektromagnesElektromagnes
KompasKompas

Materiały

3

Wymagane narzędzia

12

Według tego planu powstaje

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...