Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)
Charlie

Autor

Charlie

4. listopad 2026DE
12
0
0
0
0

Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)

The old way of getting bismuth from ore that holds it as the metal: heat the lumps just enough in sloping iron tubes and the bismuth, which melts easily, runs out of the rock into pots under charcoal. It takes 30-60 minutes a charge but gets only about two-thirds of the metal. Not given: the furnace temperature. Source: E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), Bismuth, p. 458. Picture: Thorpe's Fig. 1, the furnace in plan.
Średniozaawansowany
30-60 minutes per charge

Instrukcje

1

Pick and break the ore

Sort the ore (7-12 % bismuth) by hand from the waste rock as far as possible and break it into pieces the size of a hazel nut.

Materiały do tego kroku:

Ruda bizmutu rodzimegoRuda bizmutu rodzimego1 12 cwt per tube charge

Potrzebne narzędzia:

MłotekMłotek
Przemysłowa waga platformowaPrzemysłowa waga platformowa
2

Charge the tubes

Load about 12 cwt into each inclined iron tube of the furnace, leaving room to stir from the upper end. Close the upper ends with iron plates and the lower ends with plates pierced with round holes. Under each lower end stand an iron pot holding powdered charcoal, kept gently warm by a small charcoal fire.

Materiały do tego kroku:

Węgiel drzewnyWęgiel drzewny1 powdered, in the pots and for the pot fire

Potrzebne narzędzia:

Piec do wytapiania bizmutu (likwacji)Piec do wytapiania bizmutu (likwacji)
Tygiel żeliwnyTygiel żeliwny
3

Sweat out the bismuth

Fire the furnace with wood so that the metal flows easily. In about 10 minutes the bismuth begins to run into the pots, where the charcoal covers it from the air. Stir the ore now and then with an iron rod from the upper end; in 30-60 minutes the charge is done. 20 cwt of ore burns about 63 cubic feet of wood.

Materiały do tego kroku:

Drewno opałoweDrewno opałowe1 about 63 cu ft per 20 cwt of ore

Potrzebne narzędzia:

Piec do wytapiania bizmutu (likwacji)Piec do wytapiania bizmutu (likwacji)
Okrągły pręt żelaznyOkrągły pręt żelazny
4

Rake out and recharge

Rake the spent ore (bismuth barley) out of the upper end into the tank and refill at once with fresh ore.

Potrzebne narzędzia:

Grabie żelazneGrabie żelazne
Piec do wytapiania bizmutu (likwacji)Piec do wytapiania bizmutu (likwacji)
5

Cast ingots

Ladle the bismuth from the pots into moulds and cast ingots of 25-50 lb.

Potrzebne narzędzia:

Tygiel żeliwnyTygiel żeliwny
Kadź odlewniczaKadź odlewnicza
Kokila do wlewkówKokila do wlewków

Materiały

3

Wymagane narzędzia

8

Według tego planu powstaje

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...