Bromide Paper: Gelatino-Bromide Emulsion Coated on Paper
English
Charlie

Autor

Charlie

18. październik 2026DE
17
0
0
0
0

Bromide Paper: Gelatino-Bromide Emulsion Coated on Paper

Bromide paper is paper coated with silver bromide in gelatin, the printing and enlarging paper of the darkroom. Thorpe (1913) gives a beginner's emulsion: gelatin swelled in potassium bromide solution, silver nitrate made clear with strong ammonia, the two joined under ruby light, ripened, set, washed, and spread on paper as on a glass plate. From the moment the silver goes in, work only by ruby light. Grain and ounce figures are Thorpe's; the gram conversions and the 10-sheet batch are ours. The picture: our own drawing.
Zaawansowany
4 days

Instrukcje

1

Swell the gelatin

Dissolve 185 grains (12.0 g) of potassium bromide in 5 oz (142 ml) of water. Cover 300 grains (19.4 g) of hard gelatin with it and stir until it softens and swells.

Materiały do tego kroku:

Bromek potasuBromek potasu12 g
Żelatyna w proszkuŻelatyna w proszku19.4 g

Potrzebne narzędzia:

WodaWoda
Zlewka szklanaZlewka szklana
Bagietka szklanaBagietka szklana
Waga szalkowaWaga szalkowa
2

Dissolve the silver

Dissolve 231 grains (15.0 g) of silver nitrate in 5 oz (142 ml) of water with gentle heat in the water bath. Add strong ammonia (0.880) a little at a time, stirring, until the precipitate that first forms dissolves again.

Materiały do tego kroku:

Azotan srebraAzotan srebra15 g

Potrzebne narzędzia:

WodaWoda
Stężony roztwór amoniaku (0,880)Stężony roztwór amoniaku (0,880)
Zlewka szklanaZlewka szklana
Bagietka szklanaBagietka szklana
Duży garnekDuży garnek
3

Melt the gelatin, never above 35 °C

Stand both vessels in the pan of water, never above 35 °C, stirring, until the gelatin is perfectly liquid. Up to here ordinary light is fine.

Potrzebne narzędzia:

Duży garnekDuży garnek
TermometrTermometr
Bagietka szklanaBagietka szklana
4

Add the silver under ruby light

From now on, ruby light only. Pour the silver solution into the gelatin in a thin stream, stirring all the time. Rinse the silver beaker with about 1 oz (28 ml) of warm water into the emulsion.

Potrzebne narzędzia:

Rubinowe światło ciemnioweRubinowe światło ciemniowe
Zlewka szklanaZlewka szklana
Bagietka szklanaBagietka szklana
WodaWoda
5

Ripen

Leave the emulsion in the hot water for half to three-quarters of an hour.

Potrzebne narzędzia:

Duży garnekDuży garnek
Rubinowe światło ciemnioweRubinowe światło ciemniowe
6

Set in the dark

Pour it into a flat dish, put it in a light-tight box and let it set for at least 24 hours; two or three days is better.

Potrzebne narzędzia:

Płytkie tace ceramicznePłytkie tace ceramiczne
Skrzynka światłoszczelnaSkrzynka światłoszczelna
7

Wash through canvas

Scrape the set jelly onto wet coarse canvas and tie it into a bag. Knead it under water so it squeezes through in threads. Pour off the water, cover with fresh, wait 5 minutes and pour off: six to eight times.

Potrzebne narzędzia:

ŁopatkaŁopatka
Płótno bawełnianePłótno bawełniane
SznurekSznurek
WodaWoda
Rubinowe światło ciemnioweRubinowe światło ciemniowe
8

Drain and store

Turn the threads onto a strainer covered with a cloth and let the water drain. Rinse with methylated spirit and keep in a lidded jar until coating.

Potrzebne narzędzia:

SitkoSitko
MuślinMuślin
Alkohol skażonyAlkohol skażony
Słoiki szklane z pokrywkamiSłoiki szklane z pokrywkami
Rubinowe światło ciemnioweRubinowe światło ciemniowe
9

Coat the paper

Melt the emulsion in the warm water bath. Lay a sheet of paper flat on a levelled glass slab. Pour emulsion on the middle to cover nearly half the sheet, and spread it to each end with a glass rod 2 inches wider than the sheet, held just off the surface.

Materiały do tego kroku:

PapierPapier10 arkuszy

Potrzebne narzędzia:

Duży garnekDuży garnek
Tafla szklanaTafla szklana
PoziomicaPoziomica
Bagietka szklanaBagietka szklana
Rubinowe światło ciemnioweRubinowe światło ciemniowe
10

Dry

When the coat has set, move the sheets to a rack in a drying box with a current of air. They dry in 12 to 48 hours. Keep them in the light-tight box.

Potrzebne narzędzia:

Suszarka (regał)Suszarka (regał)
Skrzynka światłoszczelnaSkrzynka światłoszczelna

Materiały

4

Wymagane narzędzia

20

Według tego planu powstaje

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...