Carbon as Pure Graphite: Coke and Sand Heated round a Coke Core in an Electric Furnace (Acheson, US 568,323)
Charlie

Autor

Charlie

1. listopad 2026DE
0
0
0
0
0

Carbon as Pure Graphite: Coke and Sand Heated round a Coke Core in an Electric Furnace (Acheson, US 568,323)

Acheson found that carbon heated on its own hardly turns to graphite, but carbon first bound to silicon does. Coke and sand packed round a coke core form silicon carbide when the current heats the core; hotter still, the silicon boils away and the carbon is left as pure graphite, which grows outward as the core. Result: pure carbon in its graphite form, sorted like native graphite. Source: E. G. Acheson, US patent 568,323 (1896), pp. 1-3 and drawing (shown above). The furnace runs at hundreds of volts and up to 1000 amperes.
Zaawansowany
2 days

Instrukcje

1

Mix the charge

Grind and mix powdered coke, sand, salt and sawdust thoroughly, the coke about half the weight (50 parts coke to 50 parts silica and other materials).

Materiały do tego kroku:

Koks hutniczyKoks hutniczy50 parts

Potrzebne narzędzia:

PiasekPiasek
Chlorek sodu (sól)Chlorek sodu (sól)
TrocinyTrociny
Moździerz z tłuczkiemMoździerz z tłuczkiem
2

Build the furnace

Build a furnace of firebrick with carbon electrodes through the two end walls. Lay a core of granular coke between the electrodes (Acheson's was 7 ft long by 4 in wide) and pack the mixture all round it.

Materiały do tego kroku:

Koks hutniczyKoks hutniczy1 granular, for the core

Potrzebne narzędzia:

Cegły szamotoweCegły szamotowe
Elektroda grafitowaElektroda grafitowa
3

Run the current

Turn on the current, at first about 650 V and 50 A. The core heats, and silicon carbide forms round it; as the heat rises further the carbide breaks up, silicon goes off as vapour and graphite is left, carrying more current. Near the end it is about 100 V and 1000 A. Stop before the graphite reaches the walls. Ours: a step-down transformer as the supply.

Potrzebne narzędzia:

Transformator obniżający napięcieTransformator obniżający napięcie
Elektroda grafitowaElektroda grafitowa
4

Take out the graphite

When cool, separate the graphite from the core and the unchanged mixture, and grade it like native graphite.

Potrzebne narzędzia:

Moździerz z tłuczkiemMoździerz z tłuczkiem

Materiały

1

Wymagane narzędzia

7

Według tego planu powstaje

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...