Casting a Tetsubin Iron Kettle — Sand Mold Method
Forge

Created by

Forge

23. March 2026

Casting a Tetsubin Iron Kettle — Sand Mold Method

Cast a tetsubin (iron kettle) using the traditional sand-casting method practiced in Morioka and Yamagata since the Edo period. The tetsubin heats water for tea preparation and is valued for its heat retention and the trace iron it imparts to water.

Advanced
20-30 hours

Instructions

1

Create the Pattern and Core

Carve or turn a wooden pattern in the shape of the kettle exterior, split along the parting line so it can be removed from the sand mold in two halves. The pattern must be oversized by approximately 1% to account for iron shrinkage during cooling. Traditional tetsubin surfaces have a hobnail (arare) texture — press small round-headed nails into the wooden pattern surface to create the dimple impressions. Separately, create a sand core (nakago) that forms the hollow interior of the kettle. The core is made from sand mixed with a higher proportion of binder, shaped on a core box or by hand, and dried before assembly.

2

Ram the Sand Mold

Place the lower pattern half face-down in the lower flask (drag) and pack damp casting sand firmly around it using a rammer. The sand must be packed uniformly — loose areas will collapse when the pattern is withdrawn, and over-packed areas resist gas escape causing porosity in the casting. Flip the drag, place the upper pattern half on top, position the upper flask (cope) on alignment pins, and pack sand around the upper half. Insert sprue and riser pins to create channels for pouring molten iron and allowing gases to escape. Carefully separate the cope and drag, withdraw the pattern halves, and place the dried core inside the cavity. Dust all mold surfaces with graphite powder to prevent sand adhesion to the casting.

Step 2 - Image 1
3

Melt the Cast Iron

Charge the furnace with alternating layers of cast iron and coke or charcoal fuel. Cast iron melts at approximately 1150-1200 degrees C, significantly lower than steel due to its higher carbon content (2.5-4.0% C). Operate the air supply continuously. The iron is ready to pour when it flows freely and appears bright orange-white with no pasty lumps. Skim slag from the surface of the molten metal using a flat rake. The entire melt must be poured within minutes of reaching the correct temperature, as cast iron thickens rapidly once removed from the heat source.

4

Pour the Mold

Reassemble the cope and drag with the core in position, clamping or weighting them together to resist the hydrostatic pressure of molten iron. Pour the molten iron steadily into the sprue hole in a continuous stream, keeping the sprue cup full at all times. Air and gases escape through the riser channel — when molten iron appears at the riser top, the mold is full. Interrupted pouring causes cold shuts (visible seam lines where two streams of iron met but did not fuse). Allow the casting to cool in the mold for at least 4-6 hours before breaking it open.

5

Clean and Finish the Kettle

Break apart the sand mold and remove the casting. Cut off the sprue and riser stubs with a hacksaw and grind the surfaces flush. Wire-brush the entire exterior to remove adhering sand. File the lid seating surface flat so the lid sits without rocking. Traditional tetsubin are finished with a lacquer-like coating made by brewing tea inside the kettle and allowing the tannins to react with the iron surface, forming a black iron tannate layer that prevents rust and improves flavour. Forge a separate arched handle (tsuru) from wrought iron rod and attach it to cast lugs on either side of the kettle rim. Season the interior by boiling water in it three to four times before first use, discarding each batch.

Step 5 - Image 1

Materials

  • Cast iron (pig iron or scrap cast iron) - 3-4 kg piecePlaceholder
    Zobacz
  • Casting sand (fine-grained silica sand with bentonite clay binder) - 15-20 kg piecePlaceholder
    Zobacz
  • Charcoal or coke (for cupola furnace) - 10-15 kg piecePlaceholder
    Zobacz
  • Graphite or soot (mold release) - 100g piece

Wymagane narzędzia

  • Crucible or cupola furnace (capable of 1400+ degrees C)
  • Flask (two-part molding box)Placeholder
    Zobacz
  • Ladle (refractory-lined, for pouring molten iron)Placeholder
    Zobacz
  • Pattern (wooden kettle model)Placeholder
    Zobacz
  • Molding tools (rammers, trowels, sprue pins)

CC0 Public Domain

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Discussion

(0)

Log in aby dołączyć do dyskusji

Ładowanie komentarzy...