Extruded Polystyrene Foam

Carl Munters had shown that polystyrene heated with methyl chloride under pressure puffs into a closed-cell foam when let out of the vessel (US 2,023,204) - but only in small pieces; with larger outlets the mass collapsed into brittle, irregular lumps. Otis Ray McIntire at Dow found the fix: keep the mass BELOW the critical temperature of methyl chloride, about 143 °C, so the gas stays dissolved, and let its own evaporation cool the foam fast enough to freeze the cells. **US 2,450,436**, "Manufacture of cellular thermoplastic products", McIntire, assigned to Dow Chemical, filed 26. July 1947, granted 5. October 1948. Its drawing is the pressure vessel with the bottom valve the foam flows out of. Dow sold the result as blue insulation board; the white bead foam of packaging is a later process. **Methyl chloride is toxic; you start from foam board.** You build a hot-wire cutter, cut an insulated box, and measure how long it keeps ice.
Początkujący
3 hours plus an ice test

Instrukcje

1

The cutter

Base on two feet, a post and an arm; the wire runs from the arm tip down through the base to a spring underneath.
Plik projektowyBLENDCC0 - Free
2

Build the frame

From 18 mm plywood cut a 300 x 300 mm base, two 300 x 40 mm feet, a 280 x 50 mm post and a 200 x 50 mm arm. Glue and screw the post to the back edge and the arm square on top.

Materiały do tego kroku:

Płyta sklejkowaPłyta sklejkowa1 sztuka
Wkręty do drewnaWkręty do drewna10 sztuk
Klej do drewnaKlej do drewna20 ml

Potrzebne narzędzia:

Piła ręcznaPiła ręczna
Wiertarko-wkrętarka akumulatorowaWiertarko-wkrętarka akumulatorowa
Zestaw wkrętakówZestaw wkrętaków
Linijka stalowaLinijka stalowa
3

String the wire

Drill 2 mm through the arm tip and the base directly below. Fix the wire to an eye bolt on top of the arm, run it down through the base, and tie it to a spring under the base so it stays taut when it expands hot. Check it is square to the table.

Materiały do tego kroku:

Drut nichromowy 80/20 o średnicy 0,64 mmDrut nichromowy 80/20 o średnicy 0,64 mm1 metr
Śruba oczkowaŚruba oczkowa1 sztuka
Zestaw sprężyn naciskowychZestaw sprężyn naciskowych1 zestaw

Potrzebne narzędzia:

Wiertarko-wkrętarka akumulatorowaWiertarko-wkrętarka akumulatorowa
Komplet wierteł w kasecieKomplet wierteł w kasecie
4

Power it

Clip leads to the wire at the arm and below the base. Set the bench supply to 1.5 V with a 4 A limit and raise it slowly (notebook) until the wire slides through a scrap cleanly. Ventilate.

Potrzebne narzędzia:

Regulowany zasilacz warsztatowyRegulowany zasilacz warsztatowy
Alligator to Alligator CablesAlligator to Alligator Cables
Maska filtrująca N95Maska filtrująca N95
Okulary ochronne bezbarwneOkulary ochronne bezbarwne
5

Cut the box

From 25 mm foam board cut a base and lid 200 x 200 mm, two sides 200 x 150 mm and two 150 x 150 mm. Feed slowly - let the wire do the work. Tape the box together.

Materiały do tego kroku:

Płyta z polistyrenu ekstrudowanegoPłyta z polistyrenu ekstrudowanego1 arkusz
Taśma malarskaTaśma malarska1 rolka

Potrzebne narzędzia:

Linijka stalowaLinijka stalowa
6

Weigh a cube

Cut a 50 mm cube from an offcut and weigh it for the notebook.

Potrzebne narzędzia:

Cyfrowa waga kuchennaCyfrowa waga kuchenna
7

The ice test

Put 500 g of ice in a bag in the foam box and another 500 g in a cardboard box of the same size, side by side in the same room. Note the room temperature and check both every hour until the ice is gone.

Materiały do tego kroku:

Kostki loduKostki lodu1000 g
Karton falisty (pudło)Karton falisty (pudło)1 sztuka

Potrzebne narzędzia:

Cyfrowa waga kuchennaCyfrowa waga kuchenna
Termometr pokojowyTermometr pokojowy
8

Wire, density, heat leak

Wczytywanie notatnika Jupyter…
9

History & Context

**What the patent specifies:** polystyrene with methyl chloride dissolved under pressure below the gas's critical temperature, released through an outlet so evaporation expands and cools it into uniform closed cells, in blocks 2 inches thick or more. **Modern build (derived):** commercial extruded foam board, today made with other blowing agents. The patent names its target plainly: blocks big enough to cut into insulating panels for refrigerators. Its limits: it melts at low heat, burns unless treated, dissolves in many solvents (and in some glues and paints), and breaks down in sunlight.
Krok 9 - Image 1

Materiały

10

Wymagane narzędzia

11

Pliki projektowe

1

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...