Extruded Polystyrene Foam: Butylene-Blown Logs 20 Inches Across (McIntire, Dow 1948, Ex. 4)
Charlie

Autor

Charlie

28. październik 2026DE
1
0
0
0
0

Extruded Polystyrene Foam: Butylene-Blown Logs 20 Inches Across (McIntire, Dow 1948, Ex. 4)

Extruded polystyrene foam blown with a butylene gas fraction. 300 lb of polystyrene and about 130 lb of the fraction stand two days at 110 °C under 265 psi. Opened again and again, the tower let out foam logs 20 inches across and 20 feet long, weighing only 0.8 lb per cubic foot. Unknown: a source for the butylene fraction, linked to an unknown head. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 4. Picture: the patent's drawing.
Zaawansowany
3 days

Instrukcje

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Materiały do tego kroku:

PolistyrenPolistyren300 funty

Potrzebne narzędzia:

Reaktor ciśnieniowyReaktor ciśnieniowy
Waga szalkowaWaga szalkowa
Rękawice gumoweRękawice gumowe
2

Add the butylene fraction

Add about 130 lb of a cracked-oil gas fraction that is about 87 % normal butylenes, with some butanes and butadiene, under pressure. Unknown: a source for this fraction. Flammable gas: no flames, strong ventilation.

Materiały do tego kroku:

Frakcja gazu krakingowego bogata w butylenyFrakcja gazu krakingowego bogata w butyleny130 funty

Potrzebne narzędzia:

Butla na gaz pod ciśnieniemButla na gaz pod ciśnieniem
Reaktor ciśnieniowyReaktor ciśnieniowy
Gogle chemiczneGogle chemiczne
3

Heat two days at 110 °C

Close the tower and heat it at 110 °C for two days. The gauge pressure stays at 265 psi.

Potrzebne narzędzia:

Reaktor ciśnieniowyReaktor ciśnieniowy
Termometr laboratoryjnyTermometr laboratoryjny
4

Let out logs through a 3.25 inch outlet

Open and close the 3.25 inch outlet near the bottom again and again. Each portion swells into a foam log 20 inches across and about 20 feet long, with fine, even, closed cells, weighing 0.8 lb per cubic foot.

Potrzebne narzędzia:

Reaktor ciśnieniowyReaktor ciśnieniowy
Gogle chemiczneGogle chemiczne
Rękawice gumoweRękawice gumowe
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Potrzebne narzędzia:

Piła stolarskaPiła stolarska
Rękawice gumoweRękawice gumowe

Materiały

2

Wymagane narzędzia

7

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...