Fired Silver Paint: Silver Oxide and Flux in Purified Dextrin and Water (Gray, Erie Resistor 1954, Ex. 3)
Ed

Autor

Ed

28. październik 2026FI
2
0
0
0
0

Fired Silver Paint: Silver Oxide and Flux in Purified Dextrin and Water (Gray, Erie Resistor 1954, Ex. 3)

A paint for putting silver electrodes on ceramic, glass or mica. Silver oxide and a little ceramic flux are held in purified dextrin dissolved in water. The wet paint conducts electricity, so a capacitor can be measured while it is being painted. On firing, the silver oxide turns into a silver film held on by the flux. Dextrin needs no alcohol against foam, and silver nitrate does not attack it while the paint is in use. Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 3. Unknown: how the dextrin is purified. Gray does not give it. Also not given: which flux, and the firing heat. Bismuth subnitrate, one of the fluxes Gray names, is ours. Picture drawn by Youblob.
Początkujący
1 day

Instrukcje

1

Dissolve 4 g purified dextrin in the water

For 100 g of paint: dissolve 4 g purified dextrin in the water. The water is the balance, about 31 to 44 g. Unknown: how the dextrin is purified. Gray does not give it.

Materiały do tego kroku:

Dekstryna oczyszczonaDekstryna oczyszczona4 g
Woda destylowanaWoda destylowana1 as required

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Zlewka borokrzemowaZlewka borokrzemowa
Pręt ze szkła borokrzemowegoPręt ze szkła borokrzemowego
2

Grind in silver oxide and flux

Grind 50 g precipitated silver oxide and 2 to 10 g ceramic flux into the solution until smooth. Gray gives the flux only as a class; ours: bismuth subnitrate, one of the common fluxes he names. The right amount depends on the ceramic it will be fired onto.

Materiały do tego kroku:

Tlenek srebraTlenek srebra50 g
Zasadowy azotan bizmutuZasadowy azotan bizmutu1 as required

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Moździerz z tłuczkiemMoździerz z tłuczkiem
Rękawice nitryloweRękawice nitrylowe
3

Stir in up to 5 g silver nitrate

Stir in 0 to 5 g silver nitrate; it makes the wet paint conduct better. Dextrin is not attacked by it in normal use, and the paint can stand for hours without stirring. Silver nitrate stains and burns skin: gloves.

Materiały do tego kroku:

Azotan srebraAzotan srebra1 as required

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Pręt ze szkła borokrzemowegoPręt ze szkła borokrzemowego
Rękawice nitryloweRękawice nitrylowe

Materiały

5

Wymagane narzędzia

5

Według tego planu powstaje

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...