Forged Hunting Axe (Hatchet)
A small one-handed axe forged from a 7/8 × 2-inch bar of good tool steel, best made by two people; a 6¾-inch bar gives two heads. The eye, about 9/16 × 1½ inches, is punched at a yellow heat with an eye punch and opened with drifts, the blade drawn out to a 3-inch edge and the head cut to length. The axe is annealed in lime or ashes, ground and buffed, then hardened from the hardening heat in tepid water and tempered by two hot iron bars laid on either side at the centre: dark purple for the blade, blue for the head.
Zaawansowany
4–6 hours
Instrukcje
1
1
Mark and punch the eye
Mark and punch the eye
Mark the stock with chisel and centre punch. At a yellow heat, punch the eye with the narrow edge of the punch toward the blade; lift the punch after each blow to check it runs straight and to let it cool; a little fine coal in the hole stops it sticking. Punch nearly through, then finish from the other side.
Materiały do tego kroku:
Płaskownik ze stali narzędziowej1 sztukaPotrzebne narzędzia:
Punktak
Kuźnia kowalska
Kowadło
Przebijak na gorąco
Młot dwuręczny
Szczypce kowalskie2
2
Drift and draw out
Drift and draw out
Drive in a tool-steel drift, hammer the bulges down to the bar's size and smooth with a flatter; take the drift out before each reheat. Use two drifts, the first 3/8 inch narrower. Draw out the blade, driving the drift back in as the eye stretches so no cold shut forms.
Potrzebne narzędzia:
Przebijak rozszerzający
Gładzik kowalski
Młot ogoniasty3
3
Shape and trim
Shape and trim
Shape the blade with a heavy hammer and flatter and form its edge. Cut the head from the bar, draw it to size, cut it to length, then trim the blade to shape.
Potrzebne narzędzia:
Młot kowalski
Gładzik kowalski
Przecinak na gorąco4
4
Anneal and grind
Anneal and grind
Heat to a full red and anneal in lime or ashes. When cold, grind on an emery wheel and finish on a buffing wheel.
Potrzebne narzędzia:
Kuźnia kowalska
Szlifierka stołowa5
5
Harden and temper
Harden and temper
Heat very slowly to the hardening heat and cool in tepid water. Draw the temper with two hot iron bars laid on either side at the centre; when the blade is dark purple and the head blue, cool quickly in water.
Potrzebne narzędzia:
Kuźnia kowalska
Kadź hartownicza
Szczypce kowalskie6
6
Handle
Handle
Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.
Materiały do tego kroku:
Listwa z drewna twardego na trzonki1 sztuka
Klin z drewna twardego1 sztuka
Olej lniany10 mlPotrzebne narzędzia:
Strug kabłąkowy
Piła traczka
Imadło warsztatoweMateriały
4- 1 sztukaZastępnik
- Zastępnik
- 1 sztukaZastępnik
- 10 mlZastępnik
Wymagane narzędzia
16- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
Według tego planu powstaje
Powiązane blueprinty
Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami
CC0 Domena publiczna
Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.
Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.