Glass Tube: Drawn by Two Glassmakers Walking Apart (Pellatt, 1849)
Charlie

Autor

Charlie

4. listopad 2026DE
8
0
0
2
0

Glass Tube: Drawn by Two Glassmakers Walking Apart (Pellatt, 1849)

How glass tube was made by hand: a blown gather of glass is welded at one end to a second rod, and two workers walk away from each other while turning, stretching the hot glass into a tube up to 60 or 70 feet long. Because the whole bubble stretches evenly, the bore and the wall stay in the same proportion all along the tube. Result: long glass tube of nearly even bore, cut into lengths when cold. Solid cane is made the same way without blowing. Source: Apsley Pellatt, Curiosities of Glass Making (1849), pp. 106-108. Unknown: the glass batch and the gather's size. Picture: the book's figures.
Ekspert
Unknown

Instrukcje

1

Gather and blow the ball

Gather a solid ball of flint glass on the end of the blowing iron and blow it out a little, so it is hollow. When it has partly cooled, use it as a core for one or more further gatherings until there is enough glass. For flat-bore thermometer tube, flatten the first ball on the marver with an iron or wooden battledore before the later gatherings. Ours: lead crystal. Not given: the amount of glass.

Materiały do tego kroku:

Kryształ ołowiowyKryształ ołowiowy1 flint glass

Potrzebne narzędzia:

Piec szklarski osiągający 1100 stopni CelsjuszaPiec szklarski osiągający 1100 stopni Celsjusza
Piszczel hutnika szkłaPiszczel hutnika szkła
Marwer (płyta do wałkowania szkła)Marwer (płyta do wałkowania szkła)
2

Swing it long and fix the post

Lengthen the ball by swinging it, and chill its far end by dipping it in cold water. A second worker makes a disc of hot glass on a rod, the 'post', and holds it upright near the ground. The chief worker climbs onto a chair and drops the hot ball onto the post, where it welds on.

Potrzebne narzędzia:

WodaWoda
Przylepiak szklarskiPrzylepiak szklarski
3

Walk apart and draw

The chief worker steps down and the two walk away from each other, both turning their rods all the time. At first the hot glass sags between them in a curve; fan the parts that are thicker to cool them, so it stretches evenly. Draw it to the length wanted, up to 60 or 70 feet; as it cools it stops turning and pulls nearly straight. Except at the ends, it has nearly one bore, diameter and wall thickness. Ours: a wooden paddle for fanning (Pellatt: a boy's hat).

Potrzebne narzędzia:

Piszczel hutnika szkłaPiszczel hutnika szkła
Przylepiak szklarskiPrzylepiak szklarski
Wiosło drewnianeWiosło drewniane
4

Lay down and cut

Lay the tube across the wooden rungs of a ladder to cool. Cut it into lengths by touching it with a cold iron or nicking it with a steel file.

Potrzebne narzędzia:

Drabina drewnianaDrabina drewniana
Pilnik do metaluPilnik do metalu

Materiały

1

Wymagane narzędzia

8

Według tego planu powstaje

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...