Chamois Wash Leather: Frized Pelts Fulled With Fish Oil Eight or Nine Times (Morfit, 1852)
Tex

Autor

Tex

14. listopad 2026FO
5
0
0
0
0

Chamois Wash Leather: Frized Pelts Fulled With Fish Oil Eight or Nine Times (Morfit, 1852)

Oil-tawed chamois or wash leather, from Campbell Morfit's Arts of Tanning, Currying and Leather-Dressing (1852): sheep, goat or deer pelts with the grain rubbed off, beaten again and again with fish oil until it is worked right in, warmed so the oil sets in the fibre, then washed of excess oil in weak potash lye and finished soft. No tannin, no alum.
Zaawansowany
About 2 weeks

Instrukcje

1

Oil budget

Wczytywanie notatnika Jupyter…
2

Read The Arts of Tanning

"Oiled leather is commonly known as chamois, or wash-leather ... from its property of bearing wetting and washing."
3

Make pelts and friz

Choose the finest goat, sheep, lamb or deer skins (or thin split sides). Bring them to pelt as for kid leather: wash, lime, fleece, beam and bran. Then friz them: rub with a pumice stone, or work under the round edge of a blunt knife, to remove the grain, even the thickness and soften the skin.

Materiały do tego kroku:

Owcza skóraOwcza skóra12 sztuk
Wapno gaszoneWapno gaszone1 sztuka
Otręby pszenneOtręby pszenne1 sztuka

Potrzebne narzędzia:

Kadź garbarskaKadź garbarska
Kobylica do mizdrowaniaKobylica do mizdrowania
Nóż do odmięśnianiaNóż do odmięśniania
PumeksPumeks
4

Oil and full

Wring the skins and beat them in the fulling trough until nearly dry. Spread each on the table and sprinkle the grain side with cod or other fish oil, fold them in bundles of four, and beat again 2 to 4 hours. Open and air them briefly, grease again, and full again. Repeat eight or nine times until thoroughly imbued, with no greasy look. 3 to 5 gallons of oil serve a gross of skins. (By hand: beat them in a tub with a heavy wooden mallet, our method.)

Materiały do tego kroku:

Olej rybiOlej rybi1 sztuka

Potrzebne narzędzia:

Kadź garbarskaKadź garbarska
Pobijak drewnianyPobijak drewniany
5

Warm and set

Hang the skins on hooks from wooden hangers in a warm drying room (his is about 6 ft high and 12 ft square, heated by steam-pipes or a stove). A slight fermentation sets the oil into the fibre.
6

Wash out the excess

Handle the skins for an hour in slightly warm potash lye of 2 deg Baume, which turns the excess oil to soap. Wring them at the peg, dry, finish on the stretcher and the stake (horse), and smooth with rollers. For a buff colour dip them in an oak-bark infusion (a dye here, not a tan).

Materiały do tego kroku:

Wodorotlenek potasuWodorotlenek potasu1 sztuka
Kora dębowa (rozdrobniona)Kora dębowa (rozdrobniona)1 sztuka

Potrzebne narzędzia:

Kadź garbarskaKadź garbarska
Wiadro 20-litroweWiadro 20-litrowe
7

Troubleshooting

Chamois troubleshooting.

Flow

Loading...
8

History and honest limits

From Campbell Morfit, **The Arts of Tanning, Currying, and Leather-Dressing** (1852), "Oiled Leather" (checked on the archive.org scan artsoftanningcur00morf, pp. 433-436). He refers back to kid leather for the pelt stage. Hand fulling, the tools and the diagram are ours.

Materiały

6

Wymagane narzędzia

6

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...