Polypropylene Felt: a Spunbonded Web, Kinney 1967
Tex

Autor

Tex

18. październik 2026FO
10
0
0
0
0

Polypropylene Felt: a Spunbonded Web, Kinney 1967

A polypropylene felt made without weaving or needling: hot filaments are spun, pulled down by an air jet, given an electric charge so they spread apart, and laid in loops on a moving table until they form an even sheet. Kinney's patent (Du Pont, US 3,338,992, 1967) gives every setting for polypropylene. The corona runs at 20 to 25 kV: keep clear of it while it is live. The picture: the patent's own Fig. 1 (the process) and Fig. 7 (the web).
Zaawansowany
1 day

Instrukcje

1

Melt and spin

Melt polypropylene of melt index 10 in a screw extruder, no hotter than 290 °C. Meter it at 12 g a minute through a 1/4 in. sand filter and a 20-hole spinneret (holes 0.015 in. across): pack block 275 °C, spinneret 260 °C.

Materiały do tego kroku:

Granulat polipropylenowyGranulat polipropylenowy500 g

Potrzebne narzędzia:

Wytłaczarka do tworzyw sztucznychWytłaczarka do tworzyw sztucznych
Dysza przędzalniczaDysza przędzalnicza
PirometrPirometr
Waga szalkowaWaga szalkowa
Rękawice skórzaneRękawice skórzane
2

Quench

Cool the bundle of filaments in a 6 in. quench chimney blowing 40 cubic feet a minute of room air in from the side.

Potrzebne narzędzia:

Sprężarka powietrzaSprężarka powietrza
3

Draw with the air jet

Lead the bundle 72 in. down into an air draw jet run at 25 psi: it pulls the filaments with about 3 g of tension and stretches them.

Potrzebne narzędzia:

Dysza ciągnąca powietrzemDysza ciągnąca powietrzem
Sprężarka powietrzaSprężarka powietrza
ManometrManometr
4

Charge the filaments

8 in. above the jet, let the filaments brush a 1 1/4 in. bar turning at 10 rpm, with a four-point corona 5/8 in. from it at minus 20 to 25 kV (100 to 150 µA). The charge pushes them apart. Keep clear while it is live.

Potrzebne narzędzia:

Jednostka ładowania koronowegoJednostka ładowania koronowego
5

Lay the web

Catch the filaments on a grounded 47 in. square table that moves 26 in. a minute one way and 570 in. a minute the other. Each layer weighs 0.5 oz per square yard; lay several for each sheet.

Potrzebne narzędzia:

Stół układającyStół układający
6

What you get

An even sheet of fine filaments, about 2.5 denier each, tenacity 2.0 g per denier, stretching 300 % before they break.

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa

Materiały

1

Wymagane narzędzia

10

Według tego planu powstaje

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...