Pouring Temperature: Too Cold Misruns, Too Hot Tears the Mould
Forge

Autor

Forge

24. wrzesień 2026NO
14
0
0
0
0

Pouring Temperature: Too Cold Misruns, Too Hot Tears the Mould

Metal is not poured at its melting point. It is poured at a SUPERHEAT above it — enough that it can travel through the gating and fill the last thin corner before it starts to freeze. Too little superheat and the metal stops before the cavity is full, or two streams meet and fail to fuse. Too much and it dissolves more gas, oxidises harder, burns the sand, and shrinks more on the way down — so the porosity gets worse rather than better. The window is perhaps 100 to 150 degrees wide, it differs by alloy and by casting, and the only way to sit inside it reliably is to MEASURE. Judging melt temperature by colour is the pyrometer rung's warning delivered with molten metal.
Zaawansowany
3 hours

Instrukcje

1

Superheat, by alloy

Wczytywanie notatnika Jupyter…

Materiały do tego kroku:

Sztabka brązuSztabka brązu1 sztuka
Wlewek aluminiowy 99,7 % czystości, 450 gWlewek aluminiowy 99,7 % czystości, 450 g1 sztuka

Potrzebne narzędzia:

PirometrPirometr
Termopara z odczytemTermopara z odczytem
Komputer stacjonarnyKomputer stacjonarny
2

Skim, and do not stir the dross back in

Oxide and impurities float. Skim them off the surface of the melt immediately before pouring, with a preheated skimmer, and take them right out of the crucible rather than pushing them aside. Preheat every tool that will touch molten metal. A cold skimmer or ladle chills the metal locally and, far worse, any trace of moisture on it flashes to steam instantly — which throws metal. Do not stir after skimming. Stirring folds the remaining surface oxide down into the melt, where it becomes inclusions in the casting. Aluminium is the worst for this: its oxide skin is tough, and every disturbance of the surface makes more of it.

Materiały do tego kroku:

Sztabka brązuSztabka brązu1 sztuka

Potrzebne narzędzia:

Cedzak o drobnej siatceCedzak o drobnej siatce
Kadź odlewniczaKadź odlewnicza
Szczypce do tyglaSzczypce do tygla
Rękawice skórzane z długim mankietemRękawice skórzane z długim mankietem
3

Dry everything, and mean it

Water and molten metal is the one genuinely dangerous combination in a foundry. Water turned to steam expands roughly 1,600 times, instantly, and if it is under metal it throws that metal outward. So: preheat and dry the crucible, the tongs, the ladle and every ingot before it goes near the melt. An ingot with condensation on it, or a scrap casting with water trapped in a cavity, is the classic cause. The mould matters too. Green sand contains water by design and that is fine because it is bound in the clay and the mould is permeable — but a sand that is too wet, or a mould left standing so condensation collects, is the same hazard in a different place.

Materiały do tego kroku:

Sztabka brązuSztabka brązu1 sztuka
Węgiel drzewny w kawałkachWęgiel drzewny w kawałkach1 sztuka

Potrzebne narzędzia:

TygielTygiel
Szczypce do tyglaSzczypce do tygla
Przyciemniane gogle kowalskiePrzyciemniane gogle kowalskie
Rękawice skórzane z długim mankietemRękawice skórzane z długim mankietem
4

Everything ready before the metal is

Once the metal is at temperature it is losing heat and gaining gas every second. The moulds must be closed, weighted, vented and positioned before the crucible comes out of the furnace. Weight or clamp the cope. Molten metal exerts real upward pressure on the top half of the mould, and an unweighted cope lifts and lets metal run out of the parting line — which is dangerous as well as a lost casting. Have a clear path, a clear floor, and somewhere planned to put the crucible down. The pour itself takes a few seconds; everything that makes it go well or badly was decided in the minutes before it.

Materiały do tego kroku:

Piasek formierskiPiasek formierski1 kg

Potrzebne narzędzia:

Skrzynka formierska (górna i dolna)Skrzynka formierska (górna i dolna)
Szczypce do tyglaSzczypce do tygla
Przyciemniane gogle kowalskiePrzyciemniane gogle kowalskie
Rękawice skórzane z długim mankietemRękawice skórzane z długim mankietem

Materiały

4

Wymagane narzędzia

10

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...