Precipitated Silica: Hot Water Glass Carbonated, Then Acidified to pH 6.75 (Allen 1957)
Bubble carbon dioxide through hot dilute water glass and the silica comes down as an extremely fine white powder rather than a gel. Edward Allen of Columbia-Southern made it this way as a white reinforcing filler for rubber; this follows his Example XI, which gave a powder of 148 m² per gram.
Source: E. M. Allen (Columbia-Southern), US 2,805,955 (1957), Example XI. The percentages are our arithmetic; the filter, mill and indicator are ours. Picture drawn by Youblob.
Średniozaawansowany
2 days
Instrukcje
1
1
Dilute the water glass
Dilute the water glass
Take 12,850 g of sodium silicate solution holding 976 g Na2O and 3115 g SiO2 (7.6 % and 24.2 %, a silica to soda ratio of 3.19 by weight; our arithmetic). Dilute it with water to 48 litres in a stirred kettle with a heating coil and thermometer, and heat to 95 °C.
Materiały do tego kroku:
Szkło wodne (roztwór krzemianu sodu)12850 g
Woda1 as requiredPotrzebne narzędzia:
Reaktor ciśnieniowy
Mieszadło
Termometr
Waga szalkowa2
2
Carbonate for an hour
Carbonate for an hour
Bubble in pure carbon dioxide fast enough to add the theoretical amount in about 30 minutes, and keep going at that rate for about 1 hour. The slurry ends at pH 9.85.
Potrzebne narzędzia:
Dwutlenek węgla (gaz)
Reaktor ciśnieniowy
Mieszadło
Termometr
Papierek wskaźnikowy pH3
3
Filter and wash
Filter and wash
Filter the slurry and wash the cake twice with hot water.
Materiały do tego kroku:
Woda1 as requiredPotrzebne narzędzia:
Lejek Büchnera (porcelanowy)
Bibuła filtracyjna4
4
Acidify to pH 6.75
Acidify to pH 6.75
Stir the cake back into water and bring it to pH 6.75 with 400 ml of 3.5 N hydrochloric acid.
Materiały do tego kroku:
Woda1 as requiredPotrzebne narzędzia:
Kwas solny
Naczynie szklane
Mieszadło
Papierek wskaźnikowy pH5
5
Wash out the chloride
Wash out the chloride
Filter again and wash the cake with hot water until it is nearly free of chloride.
Materiały do tego kroku:
Woda1 as requiredPotrzebne narzędzia:
Lejek Büchnera (porcelanowy)
Bibuła filtracyjna6
6
Dry at 105 °C and grind
Dry at 105 °C and grind
Dry it at 105 °C in a fan oven and grind it to a fine powder. Allen's had a pH of 8.2, 0.61 % sodium and a surface area of 148 m² per gram.
Potrzebne narzędzia:
Piec do suszenia
Moździerz z tłuczkiem
Słoiki szklane z pokrywkamiWymagane narzędzia
13- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
- Zastępnik
Według tego planu powstaje
Powiązane blueprinty
Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami
CC0 Domena publiczna
Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.
Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.