PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)
Charlie

Autor

Charlie

28. październik 2026DE
3
0
0
0
0

PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)

A PTFE dispersion is stable on the shelf, but stirred hard enough it curdles. Fifty seconds at 1000 rpm in a baffled beaker and the polymer floats up as a dry-looking, unwettable crumb. Washed and dried, it is a free-flowing powder for rolling into tape, or for cold lubricated extrusion. Source: J. F. Lontz (du Pont), US 2,593,583 (1952), Example 1. Lontz started from a dispersion made with disuccinic acid peroxide; ours is Berry's persulfate dispersion, diluted to his 17 %. Picture drawn by Youblob.
Średniozaawansowany
1 day

Instrukcje

1

Dilute the dispersion to 17 %

Ours: stir the 34 % dispersion with an equal weight of distilled water to get 17 % solids, the strength Lontz used.

Materiały do tego kroku:

Wodna dyspersja PTFEWodna dyspersja PTFE1 part
Woda destylowanaWoda destylowana1 part

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Słoiki szklane z pokrywkamiSłoiki szklane z pokrywkami
2

Set up the baffled beaker

A 1-gallon stainless beaker, 6.5 in across and 7.5 in deep, with four baffles about ⅜ × 1 in hanging from the cover to within 3 in of the bottom. Stirrer: open turbine, 4 blades 1½ in high, 5 in across, reaching to within 1 in of the bottom.

Potrzebne narzędzia:

Zbiornik z mieszadłem i przegrodamiZbiornik z mieszadłem i przegrodami
MieszadłoMieszadło
3

Stir hard at 176 °F for 50 seconds

Put in half a gallon of the 17 % dispersion and heat it to 176 °F (80 °C). Run the stirrer at 1000 rpm for 50 seconds (Lontz measured 0.72 hp per gallon). The polymer coagulates and floats, unwetted, on top.

Potrzebne narzędzia:

Zbiornik z mieszadłem i przegrodamiZbiornik z mieszadłem i przegrodami
MieszadłoMieszadło
Płyta grzejnaPłyta grzejna
TermometrTermometr
4

Wash hot, then cold

Pour off the water. Wash the polymer with hot water at 176 °F, then with cold water at 60 °F (16 °C), and drain.

Potrzebne narzędzia:

Zbiornik z mieszadłem i przegrodamiZbiornik z mieszadłem i przegrodami
TermometrTermometr
5

Dry at 230 °F for 16 hours

Spread the wet polymer on a 100-mesh screen and dry it in an oven at 230 °F (110 °C) for 16 hours. It comes out a free-flowing granular powder that passes 6–8 mesh.

Potrzebne narzędzia:

Sito z drobnej siatki drucianejSito z drobnej siatki drucianej
Piec do suszeniaPiec do suszenia
Słoiki szklane z pokrywkamiSłoiki szklane z pokrywkami

Materiały

2

Wymagane narzędzia

8

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...