Rubber Stoppers: Pará Rubber with Ceresine, Moulded and Cured (Heil & Esch 1909)
Heil and Esch · Public domain (1909)
Emma

Autor

Emma

27. październik 2026SE
2
0
0
0
0

Rubber Stoppers: Pará Rubber with Ceresine, Moulded and Cured (Heil & Esch 1909)

Laboratory rubber stoppers from a 1909 rubber factory's book of mixings: Pará rubber with ceresine wax, sulphur and magnesia, run out as a cord, cut to weight, pressed into moulds and cured. Source: Heil & Esch, The Manufacture of Rubber Goods (1909), mixing No. 34 (p. 108) and the stopper method (p. 135). They give no cure time or temperature. Using smoked ball rubber as their Pará, and the mill, clamps and steam vessel, are ours. Picture: their page of mixings.
Średniozaawansowany
1 day

Instrukcje

1

Weigh mixing No. 34

Weigh out 10,000 g Pará rubber, 2,000 g ceresine, 1,000 g sulphur and 100 g calcined magnesia (magnesia usta).

Materiały do tego kroku:

Wędzona kula kauczukuWędzona kula kauczuku10000 g
Wosk cerezynowyWosk cerezynowy2000 g
Siarka w proszkuSiarka w proszku1000 g
Tlenek magnezuTlenek magnezu100 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
2

Mix on the rolls

Work the rubber on the mixing rolls and work the ceresine, sulphur and magnesia into it until the mixing is even.

Potrzebne narzędzia:

Walcarka dwuwalcowa do gumyWalcarka dwuwalcowa do gumy
3

Run a cord on the tube machine

Run the mixing through the tube machine as a cord of a size to suit the stoppers. It must be free from air bubbles, or the stoppers will be faulty after curing.

Potrzebne narzędzia:

Wytłaczarka do gumyWytłaczarka do gumy
4

Cut pieces to weight

Cut the cord into pieces of the exact weight of one stopper plus 2 or 3 per cent, for what squeezes out of the mould.

Potrzebne narzędzia:

Nóż introligatorskiNóż introligatorski
Waga szalkowaWaga szalkowa
5

Press into moulds and clamp

Press each piece into a mould and clamp the small moulds very tightly in iron clips.

Potrzebne narzędzia:

Forma wulkanizacyjnaForma wulkanizacyjna
Ścisk typu CŚcisk typu C
6

Cure in steam

Cure the clamped moulds in a steam heater (Heil & Esch also name the sulphur bath). They give no time or temperature for stoppers; then open the moulds and take out the stoppers.

Potrzebne narzędzia:

Autoklaw stołowyAutoklaw stołowy
Forma wulkanizacyjnaForma wulkanizacyjna

Materiały

4

Wymagane narzędzia

7

Według tego planu powstaje

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...