Neodymium Magnets, Sample 19: 79Fe-8B-13Nd Sintered (Sagawa 1988)
Forge

Autor

Forge

28. październik 2026NO
2
0
0
0
0

Neodymium Magnets, Sample 19: 79Fe-8B-13Nd Sintered (Sagawa 1988)

Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 19, 79 % iron, 8 % boron and 13 % neodymium by atoms: 29.3 MGOe. Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Ekspert
2 days

Instrukcje

1

Weigh sample 19: 79 Fe, 8 B, 13 Nd

Sample 19 is 79 % iron, 8 % boron and 13 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 640.0 g iron, 70.0 g ferroboron, 294.2 g neodymium. Unknown: how these three are made.

Materiały do tego kroku:

Żelazo elektrolityczneŻelazo elektrolityczne640 g
ŻelazoborŻelazobor70 g
Neodym metalicznyNeodym metaliczny294.2 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
2

Melt by high frequency in argon and cast

Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.

Potrzebne narzędzia:

Piec indukcyjnyPiec indukcyjny
Tygiel z gliny ogniotrwałejTygiel z gliny ogniotrwałej
ArgonArgon
Butla na gaz pod ciśnieniemButla na gaz pod ciśnieniem
Wlewnica miedziana chłodzona wodąWlewnica miedziana chłodzona wodą
Rękawice żaroodporneRękawice żaroodporne
3

Stamp to 35 mesh, ball-mill to 3-10 µm

Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.

Potrzebne narzędzia:

Stępa rudnaStępa rudna
Zestaw sit (oczka stopniowane)Zestaw sit (oczka stopniowane)
Żelazny młyn kulowyŻelazny młyn kulowy
Okulary ochronneOkulary ochronne
4

Press in a 10 kOe field at 1.5 t/cm²

Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.

Potrzebne narzędzia:

Prasa z polem magnetycznymPrasa z polem magnetycznym
5

Sinter in argon at 1000-1200 °C

Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 19 measured 13.1 kG remanence, 4.8 kOe coercivity and 29.3 MGOe.

Potrzebne narzędzia:

Piec rurowyPiec rurowy
ArgonArgon
Butla na gaz pod ciśnieniemButla na gaz pod ciśnieniem
Rękawice żaroodporneRękawice żaroodporne
6

Magnetise the magnets

Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.

Potrzebne narzędzia:

Nieznana metoda magnesowaniaNieznana metoda magnesowania

Materiały

3

Wymagane narzędzia

14

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...