Strontium Ferrite Disc Magnet: 0.4 mol SrCO3 to 3.6 mol Iron Oxide, 1270 °C (Went, Philips 1956, Ex. 14)
Charlie

Autor

Charlie

28. październik 2026DE
0
0
0
0
0

Strontium Ferrite Disc Magnet: 0.4 mol SrCO3 to 3.6 mol Iron Oxide, 1270 °C (Went, Philips 1956, Ex. 14)

A ceramic magnet with strontium in place of barium: 0.4 mol strontium carbonate to 3.6 mol iron oxide, milled 15 hours and passed through a 1270 °C furnace in 20 minutes. Went's rod held 1,290 gauss with a coercive force of 3,080 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 14. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Zaawansowany
2 days

Instrukcje

1

Weigh strontium carbonate and iron oxide

Weigh 59.1 g strontium carbonate (0.4 mol) and 580.0 g ferric oxide (3.6 mol).

Materiały do tego kroku:

Węglan strontuWęglan strontu59.1 g
Tlenek żelaza(III)Tlenek żelaza(III)580 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Półmaska P100Półmaska P100
2

Mill with alcohol 15 hours and dry

Grind with alcohol in a ball mill for 15 hours and dry.

Potrzebne narzędzia:

Żelazny młyn kulowyŻelazny młyn kulowy
Etanol - klasa laboratoryjna, 95 %Etanol - klasa laboratoryjna, 95 %
Piec do suszeniaPiec do suszenia
3

Form the pieces and dry overnight

The patent extrudes rods; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry overnight.

Potrzebne narzędzia:

Prasa hydraulicznaPrasa hydrauliczna
Matryca do prasowania krążkówMatryca do prasowania krążków
Piec do suszeniaPiec do suszenia
4

Pass through a 1270 °C zone in 20 minutes

Sinter in air at 1270 °C by passing the pieces through a 10 cm hot zone at 5 mm per minute: 20 minutes in the heat.

Potrzebne narzędzia:

Piec rurowyPiec rurowy
Rękawice żaroodporneRękawice żaroodporne
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Potrzebne narzędzia:

ElektromagnesElektromagnes
KompasKompas

Materiały

2

Wymagane narzędzia

11

Według tego planu powstaje

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...