Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)
Woody

Autor

Woody

28. październik 2026NO
3
0
0
0
0

Guitar Strings: Bronze Wound on Steel, Then Heat-Soaked (Stone and Falcone 1977)

A wound string is a steel core with another wire wrapped round it. Stone and Falcone believed the wrap keeps stresses from the winding and slowly unwinds as the string is played, so the tone goes dead. Their fix: after winding, heat-soak the string, at least 2 hours at 270 °F or 30 minutes at 480 °F for a bronze wrap, then let it cool. Source: W. N. Stone and A. S. Falcone (National Musical String Co.), US 4,063,674 (1977). Unknown: the winding itself (the patent calls it conventional), where phosphor bronze wire comes from, and the gauges. These are linked to unknown heads. The plain strings of the set are steel music wire; that, the oven and the nitrogen are ours. Picture drawn by Youblob.
Zaawansowany
1 day

Instrukcje

1

Cut the core and plain strings

Cut steel music wire for the cores of the wound strings and for the plain strings of the set. Unknown: the gauges and lengths, and the ball ends.

Materiały do tego kroku:

Stalowy drut sprężynowy 0,032"Stalowy drut sprężynowy 0,032"1 as required

Potrzebne narzędzia:

Obcinaki boczneObcinaki boczne
Nieznane wymiaryNieznane wymiary
2

Wind the bronze wrap at room temperature

Wrap phosphor bronze wire helically round each core at room temperature. The patent prefers a wrap that expands more with heat than the core. Unknown: how; the patent says only 'in a conventional manner'.

Materiały do tego kroku:

Drut z brązu fosforowegoDrut z brązu fosforowego1 as required

Potrzebne narzędzia:

Nieznana metoda nawijaniaNieznana metoda nawijania
Nieznane wymiaryNieznane wymiary
Okulary ochronneOkulary ochronne
3

Heat-soak the wound strings

Heat the wound strings for a bronze wrap at 270-480 °F (132-249 °C): at least 2 hours at 270 °F or at least 30 minutes at 480 °F, shorter the hotter. If the wire tarnishes in hot air, do it without air, in nitrogen or carbon dioxide. The wrap's turns settle into more even spacing.

Potrzebne narzędzia:

PiekarnikPiekarnik
Termometr laboratoryjnyTermometr laboratoryjny
Butla z azotemButla z azotem
4

Cool and set up the set

Let the strings cool back to room temperature. Make up the set with the plain steel strings.

Potrzebne narzędzia:

Obcinaki boczneObcinaki boczne

Materiały

2

Wymagane narzędzia

7

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...