Metal Oxide Varistor: Zinc Oxide, 0.5 % Bismuth Oxide, 1 % Antimony Trioxide, 1350 °C (Masuyama 1972, Ex. 2)
Ed

Autor

Ed

28. październik 2026FI
1
0
0
0
0

Metal Oxide Varistor: Zinc Oxide, 0.5 % Bismuth Oxide, 1 % Antimony Trioxide, 1350 °C (Masuyama 1972, Ex. 2)

Masuyama, Matsuoka and Nishi found that adding a second oxide to zinc oxide and bismuth oxide changes the varistor a great deal. This is their Example 2 with antimony trioxide: 98.5 % zinc oxide, 0.5 % bismuth oxide and 1.0 % antimony trioxide by moles, sintered at 1350 °C. The disc measured a C-value of 75 at 1 mA and a nonlinearity exponent n of 15.3. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 2. Unknown: how the aluminium is sprayed on and what the silver paint is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Zaawansowany
1 day

Instrukcje

1

Weigh 98.5 : 0.5 : 1 and wet-mill 5 hours

Mix zinc oxide, bismuth oxide and antimony trioxide 98.5 : 0.5 : 1 by moles. Ours, for 10 g: 9.386 g zinc oxide, 0.273 g bismuth oxide, 0.341 g antimony trioxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.

Materiały do tego kroku:

Proszek tlenku cynkuProszek tlenku cynku9.386 g
Tlenek bizmutuTlenek bizmutu0.273 g
Tritlenek antymonuTritlenek antymonu0.341 g

Potrzebne narzędzia:

Waga szalkowaWaga szalkowa
Żelazny młyn kulowyŻelazny młyn kulowy
Piec do suszeniaPiec do suszenia
2

Press discs 13 mm by 2.5 mm

Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm², as in Example 1.

Potrzebne narzędzia:

Prasa hydraulicznaPrasa hydrauliczna
Matryca do prasowania krążkówMatryca do prasowania krążków
SuwmiarkaSuwmiarka
3

Sinter 1 hour at 1350 °C and furnace-cool

Sinter the discs in air for 1 hour at 1350 °C, then let them cool in the furnace to room temperature (about 15-30 °C).

Potrzebne narzędzia:

Piec muflowyPiec muflowy
4

Lap to 10 mm by 1.5 mm

Lap both faces with 600-mesh silicon carbide. The finished disc is 10 mm across and 1.5 mm thick.

Potrzebne narzędzia:

Ścierniwo z węglika krzemuŚcierniwo z węglika krzemu
SuwmiarkaSuwmiarka
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.

Materiały do tego kroku:

Wlewek aluminiowyWlewek aluminiowy1 as required
Srebrna farba przewodzącaSrebrna farba przewodząca1 as required
Drut miedzianyDrut miedziany2 sztuk

Potrzebne narzędzia:

Nieznana metoda natryskiwania metaluNieznana metoda natryskiwania metalu
SuwmiarkaSuwmiarka

Materiały

6

Wymagane narzędzia

9

Powiązane blueprinty

Te blueprinty dzielą się wiedzą — technikami, materiałami lub zasadami

CC0 Domena publiczna

Ten plan jest udostępniany na licencji CC0. Możesz go swobodnie kopiować, modyfikować, rozpowszechniać i wykorzystywać do dowolnych celów, bez konieczności uzyskiwania zgody.

Wesprzyj Makera kupując produkty przez jego plan, za co zarabia Prowizja Makera ustalony przez sprzedawców, lub stwórz nową iterację tego planu i dołącz go jako połączenie w swoim własnym planie, aby dzielić się przychodami.

Dyskusja

(0)

Zaloguj się aby dołączyć do dyskusji

Ładowanie komentarzy...