Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)
Charlie

Создано

Charlie

4. ноябрь 2026DE
6
0
0
0
0

Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)

The old way of getting bismuth from ore that holds it as the metal: heat the lumps just enough in sloping iron tubes and the bismuth, which melts easily, runs out of the rock into pots under charcoal. It takes 30-60 minutes a charge but gets only about two-thirds of the metal. Not given: the furnace temperature. Source: E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), Bismuth, p. 458. Picture: Thorpe's Fig. 1, the furnace in plan.
Средний
30-60 minutes per charge

Инструкции

1

Pick and break the ore

Sort the ore (7-12 % bismuth) by hand from the waste rock as far as possible and break it into pieces the size of a hazel nut.

Материалы для этого шага:

Руда самородного висмутаРуда самородного висмута1 12 cwt per tube charge

Необходимые инструменты:

МолотокМолоток
Промышленные платформенные весыПромышленные платформенные весы
2

Charge the tubes

Load about 12 cwt into each inclined iron tube of the furnace, leaving room to stir from the upper end. Close the upper ends with iron plates and the lower ends with plates pierced with round holes. Under each lower end stand an iron pot holding powdered charcoal, kept gently warm by a small charcoal fire.

Материалы для этого шага:

Древесный угольДревесный уголь1 powdered, in the pots and for the pot fire

Необходимые инструменты:

Печь для ликвации висмутаПечь для ликвации висмута
Чугунный тигельЧугунный тигель
3

Sweat out the bismuth

Fire the furnace with wood so that the metal flows easily. In about 10 minutes the bismuth begins to run into the pots, where the charcoal covers it from the air. Stir the ore now and then with an iron rod from the upper end; in 30-60 minutes the charge is done. 20 cwt of ore burns about 63 cubic feet of wood.

Материалы для этого шага:

ДроваДрова1 about 63 cu ft per 20 cwt of ore

Необходимые инструменты:

Печь для ликвации висмутаПечь для ликвации висмута
Круглый железный прутокКруглый железный пруток
4

Rake out and recharge

Rake the spent ore (bismuth barley) out of the upper end into the tank and refill at once with fresh ore.

Необходимые инструменты:

Железные граблиЖелезные грабли
Печь для ликвации висмутаПечь для ликвации висмута
5

Cast ingots

Ladle the bismuth from the pots into moulds and cast ingots of 25-50 lb.

Необходимые инструменты:

Чугунный тигельЧугунный тигель
Литейный ковшЛитейный ковш
ИзложницаИзложница

Материалы

3

Требуемые инструменты

8

По этому чертежу делают

CC0 Общественное достояние

Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.

Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.

Обсуждение

(0)

Войти чтобы присоединиться к обсуждению

Загрузка комментариев...