Bouncing Putty
Looking for a synthetic rubber during the Second World War, James Wright at General Electric heated silicone oil with boric acid. The result was no rubber: it bounced, shattered under a hammer, stretched like toffee when pulled slowly and slumped into a puddle overnight. Nobody found an industrial use; in 1950 it was sold as a toy.
**US 2,541,851**, "Process for making puttylike elastic plastic, siloxane derivative composition containing zinc hydroxide", Wright, assigned to General Electric, filed 23. December 1944, granted 13. February 1951: liquid dimethylsiloxane heated with 5 to 25 % by weight of a boron compound such as boric acid or borax.
**You measure both of its lives**: how high it bounces, how fast it flows, and where one turns into the other.
Начинающий
1 hour plus a day of slumping
Инструкции
1
1
Weigh a ball
Weigh a ball
Weigh out 20 g of bouncing putty and roll it into a smooth ball between your palms.
Материалы для этого шага:
Прыгающая замазка20 гНеобходимые инструменты:
Прецизионные цифровые весы2
2
Bounce it
Bounce it
Tape a tape measure up a wall. Drop the ball from 1.0 m onto a hard floor five times, filming in slow motion, and read each rebound height.
Материалы для этого шага:
Малярная лента1 рулонНеобходимые инструменты:
Рулетка
Смартфон с замедленной видеосъёмкой3
3
Pull slow, pull fast
Pull slow, pull fast
Roll a 10 mm thick rope. Pull one over 10 seconds: it strings out. Pull another sharply: it snaps with a clean face. Try pull times in between and note the fastest pull that still stretches.
Необходимые инструменты:
Секундомер
Металлическая линейка4
4
Strike it
Strike it
Glasses on. Set a ball on a hard surface and hit it once, sharply, with the mallet. It cracks rather than squashing. Squash another slowly with your thumb.
Необходимые инструменты:
Резиновая киянка
Прозрачные защитные очки5
5
Let it slump
Let it slump
Re-roll the 20 g ball and set it on wax paper on a level surface. Measure its diameter now and after 10, 30, 60 and 180 minutes and 24 hours.
Материалы для этого шага:
Вощёная бумага1 листНеобходимые инструменты:
Цифровой штангенциркуль 6 дюймов6
6
Deborah numbers
Deborah numbers
Загрузка блокнота Jupyter…
7
7
History & Context
History & Context
**What the patent specifies:** liquid dimethylsiloxane heated with 5–25 % of a boron compound until putty-like. **Modern build (derived):** commercial bouncing putty, measured.
It became a famous toy and a staple of physics teaching about materials that are neither simply solid nor simply liquid. Its limits: it picks up dirt, will not hold a shape, and flows out of any container that is not closed.
Материалы
3- Заполнитель
- 1 рулонЗаполнитель
- 1 листЗаполнитель
Требуемые инструменты
8- Заполнитель
- 1 vendor sell this, none ship to you yetЗаполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
Связанные чертежи
Эти чертежи делятся знаниями — техники, материалы или принципы
CC0 Общественное достояние
Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.
Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.