Copper Concentrate: Sulphide Ore Stamped, Jigged and Tabled at the Anaconda Mill (Richards, Ore Dressing 1903)
Copper sulphide ore is too lean to smelt as mined. At the Anaconda mill it was screened, crushed under steam stamps, sorted by settling speed in rising water, and run over jigs and slime tables, where the heavy copper minerals sink and the light quartz and feldspar wash away.
Result: concentrates of 12 to 20 % copper; 100 tons of ore gave 50 to 75 tons. The mill handled 2,500 to 2,700 tons a day.
Source: Robert H. Richards, Ore Dressing vol. II (1903), pp. 984-986, Mill No. 42, Anaconda Copper Mining Company. Not given: the copper in the ore, water per ton. Picture drawn by Youblob.
Продвинутый
1 day
Инструкции
1
1
Sort the ore
Sort the ore
In the mine, pick the ore by hand into rich ore (straight to the smelter), hard concentrating ore and soft concentrating ore. The ore holds chalcocite, chalcopyrite, pyrite, enargite and blende in quartz and decomposed feldspar; the aim is to save the copper and silver without the zinc.
Материалы для этого шага:
Сульфидная медная руда100 tons2
2
Screen and pick
Screen and pick
Pass each kind over vibrating grizzlies with 1 in spaces; hand-pick the oversize for rich ore. Screen the undersize in trommels: 6.35 mm round holes for hard ore; 12.7 mm then 6.35 mm for soft ore.
Необходимые инструменты:
Классификационное сито
Барабанный грохот (бутара)3
3
Crush under steam stamps
Crush under steam stamps
Crush the coarse hard ore under steam stamps with screens of 4.76 x 9.52 mm slots, the soft ore under stamps with 12.7 mm round holes. Richards notes that steam stamps were later given up for these ores.
Необходимые инструменты:
Толчейная мельница
Вода4
4
Classify and jig
Classify and jig
Jig the coarse soft ore on 1-sieve Harz jigs. Send all fine ore to hydraulic classifiers with three spigots; each spigot feeds its own row of 2-sieve Collom jigs. The heavy concentrate is drawn from the jigs; middlings are crushed again.
Необходимые инструменты:
Отсадочная машина
Гидравлический классификатор
Вода5
5
Table the slimes and collect
Table the slimes and collect
Run the classifier overflow over convex revolving slime tables. Gather all concentrates and settlings for the smelter: 12 to 20 % copper, 50 to 75 tons from 100 tons of ore. Tailings keep 1 1/4 to 2 % copper.
Необходимые инструменты:
Вращающийся шламовый стол
ОтстойникМатериалы
1- 100 tonsЗаполнитель
Требуемые инструменты
8- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
По этому чертежу делают
CC0 Общественное достояние
Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.
Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.